| HS Code | 414343 |
| Density | 0.918 g/cm³ |
| Melt Flow Rate | 3.5 g/10 min |
| Tensile Strength At Yield | 10 MPa |
| Tensile Strength At Break | 25 MPa |
| Elongation At Break | 800% |
| Flexural Modulus | 240 MPa |
| Vicat Softening Point | 90 °C |
| Melting Point | 120 °C |
| Hardness Shore D | 50 |
| Film Haze | 10% |
| Film Gloss | 80% |
| Dart Drop Impact | 150 g |
| Tear Strength Md | 250 g |
| Tear Strength Td | 350 g |
As an accredited LyondellBasell Icorene 1041 YEW 2182 Polyethylene, Linear Low Density factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell Icorene 1041 YEW 2182 LLDPE is supplied in 25 kg polyethylene bags, typically stacked on pallets for industrial use. |
| Container Loading (20′ FCL) | Container loading (20′ FCL) of LyondellBasell Icorene 1041 YEW 2182 Linear Low Density Polyethylene, 25 kg bags, securely stowed. |
| Shipping | LyondellBasell Icorene 1041 YEW 2182 Polyethylene, Linear Low Density is a non-hazardous thermoplastic resin. Ship in 25 kg bags, octabins, or bulk containers. Store dry, away from heat and sunlight. Not regulated by DOT, IMDG, or IATA; no UN number, hazard class, or packing group required. |
| Storage | Store LyondellBasell Icorene 1041 YEW 2182 Polyethylene, Linear Low Density in a cool, dry, well-ventilated area, away from direct sunlight, heat, sparks, and open flames. Keep original containers tightly closed to prevent moisture and contamination. Separate from strong oxidizers. Avoid dust generation; use grounding/bonding where required. Maintain clean, labeled containers and comply with local storage regulations. |
| Shelf Life | Store in a cool, dry place in original unopened packaging; typical shelf life is 24 months from the production date. |
High-load-bearing tank shells produced by biaxial rotational molding in carousel equipment subject the supplied Icorene 1041 YEW 2182 linear low-density polyethylene powder to a sintering plateau between 185°C and 210°C internal air temperature. The powder is dry-blended in a high-intensity mixer at 1,200–1,600 rpm for 90–120 s; additive loading comprises 0.20–0.35 wt% hindered amine light stabilizer, 0.10–0.15 wt% phosphite antioxidant, and where outdoor ultraviolet exposure is specified, 2.0–2.5 wt% furnace carbon black. The blend is charged into cast aluminum or fabricated carbon steel molds mounted on a carousel arm with a 4:1 biaxial speed ratio. Oven set point is held at 290–315°C until the part’s mold surface reaches 230–260°C; peak internal air temperature must be maintained for 5–10 min to achieve void collapse and full densification. Pre-drying to ≤0.05 wt% moisture is required when ambient relative humidity exceeds 60%, because water vapor trapped in the melt produces pinhole defects along the wall’s outer skin. The process is bounded at the upper end by oxidative degradation: residence beyond 30 min at oven temperatures above 315°C shifts the melt toward crosslinking, yellowing, and embrittlement, while early release before the 185°C internal air threshold leaves unmelted powder pockets at mold corners. Compliance for non-potable chemical storage shells is governed by ASTM D1998-21; food-contact liners require FDA 21 CFR 177.1520(c) 3.1a and EU 10/2011 with overall migration ≤10 mg/dm². Terminal product types include vertical storage tanks of 500–10,000 L, 200 L conical hoppers, and agricultural sprayer reservoirs. Published grade-specific sintering data for this exact YEW 2182 configuration under biaxial rotation is limited; incoming lot qualification should therefore include melt flow rate measurement at 190°C/2.16 kg per ISO 1133-1:2022 and environmental stress crack resistance tracking per ASTM D1693 against the approved lot baseline.
| Control point | Standard / regulation | Evaluation target |
|---|---|---|
| Polyethylene tank wall design | ASTM D1998-21 | wall thickness and design stress per standard equations |
| Food-contact liner conformance | FDA 21 CFR 177.1520(c) 3.1a | olefin polymer extractives and end-use temperature restrictions |
| EU plastics food-contact migration | EU 10/2011 | overall migration ≤10 mg/dm² |
| Melt flow rate | ISO 1133-1:2022 | supplier datasheet value confirmed at 190°C/2.16 kg |
| Density | ASTM D792-20 | supplier datasheet value confirmed at 23°C |
| Environmental stress crack resistance | ASTM D1693 | failure time compared against approved-lot baseline |
In heavy-duty sack extrusion, the high zero-shear viscosity of linear low-density polyethylene relative to low-density polyethylene narrows the melt-fracture-free die rate. Melt temperatures at the adapter are set to 195–215°C, with die gap maintained at 1.4–1.8 mm and blow-up ratio between 2.0 and 2.5. To suppress sharkskin at output rates above 1.0 kg/mm die circumference per hour, a fluoropolymer processing aid is incorporated at 200–500 ppm, and low-density polyethylene is dry-blended at 15–20 wt%. The film layer is formulated from 80–85 wt% Icorene 1041 YEW 2182 LLDPE, 15–20 wt% LDPE, erucamide slip at 300–600 ppm, and synthetic silica antiblock at 1,000–2,000 ppm. Frost line position is held at 5–7 die diameters above the die face, using a dual-lip air ring supplied with chilled air at 7–10°C. If the frost line rises above 8 die diameters, bubble side-to-side oscillation increases and edge creasing appears in the collapsed film, while a frost line below 4 die diameters reduces transverse direction dart impact because crystallization completes too rapidly. Packaging waste regulation EU 94/62/EC and REACH 1907/2006 apply to the finished sack; mechanical acceptance is measured against ISO 7765-1:2014 puncture and ASTM D1709-16a dart drop, with tensile elongation per ISO 527-3. The terminal product is a 25 kg heavy-duty sack for polymer pellets, fertilizers, and fine chemical powders where weld seam integrity at the spout and side gusset stress resistance are required.
Three-layer coextrusion of a 180–200 µm greenhouse cover imposes a multi-year ultraviolet durability requirement that shifts the additive package from processing aids to light stabilizers. In the core layer, 100 parts of the LLDPE resin is combined with 0.5–0.8 wt% high-molecular-weight HALS, 0.2–0.5 wt% ultraviolet absorber, and 5–15 wt% ethylene-vinyl acetate for infrared retention and mechanical damping. The inner surface layer receives 0.1–0.3 wt% nonionic antifog concentrate to reduce pendant droplet formation. The extrusion line operates with a die lip gap of 1.2–2.0 mm, blow-up ratio 2.5–3.2, and melt temperature 190–210°C; a tower height of 12–16 m is used to maintain bubble stability and prevent blocking in the collapsing frame. The finished film is conformity assessed under EN 13206:2017 for thermoplastic agricultural films; where the structure is exported to markets with strict substance screening, RoHS 2011/65/EU cadmium-free stabilizer verification may also be required. Bubble stability in wide-web lines is highly sensitive to ambient air velocity; side-wall draft greater than 2 m/s causes gauge variation exceeding ±10% measured by ISO 4593-2. The terminal product is multi-season greenhouse cladding film, low-tunnel cover, and silage protection sheeting, each supplied in roll lengths of 100–500 m. Published data for the specific YEW 2182 grade in a three-layer agricultural film stack is limited; the above formulation represents industrial practice for LLDPE stabilized greenhouse film based on ISO 4892-2 accelerated weathering benchmarks.
Where a three-layer polyolefin coating is specified for buried steel line pipe, the outer LLDPE shield is extruded at 190–230°C through a crosshead die onto an adhesion layer that has been co-extruded or spiral-wrapped over a fusion-bonded epoxy base. The steel surface is grit-blast cleaned to Sa 2.5 per ISO 8501-1 and preheated to 170–200°C before the 100–150 µm epoxy layer is applied; the intermediate maleic anhydride grafted adhesive must remain within 0.2–0.4 mm to prevent disbondment under cathodic protection. The LLDPE topcoat is formulated with 2.0–2.5 wt% carbon black for ultraviolet protection, 0.15–0.25 wt% hindered phenol antioxidant, and 0.20–0.30 wt% HALS to resist oxidative embrittlement in above-ground storage. Total topcoat thickness is 2.5–3.5 mm, with tensile properties determined per ASTM D638-14 and coating qualification per ISO 21809-1:2018. The primary processing constraint is steel preheat temperature: below 170°C, the adhesive does not activate sufficiently; above 210°C, the epoxy base can oxidize and the LLDPE layer can develop gel specks from residence-time-induced crosslinking in the transfer adapter. Coated pipe is quenched in 60–80°C water to avoid vacuum void formation at the steel–epoxy interface. The terminal product is 3LPE-coated line pipe in grades X52–X70 for oil and gas gathering networks, where the LLDPE layer functions as the mechanical shield against soil stress and rock indentation.
Cast stretch film made in a high-velocity chill-roll line is a high-volume LLDPE application where the film’s cling force and puncture resistance are developed without machine-direction orientation. Melt temperature is held at 240–260°C, die gap at 0.4–0.8 mm, air gap at 10–20 mm, and chill roll temperature at 15–25°C; line speed exceeds 600 m/min on wide-web cast lines. The formulation uses 100 parts of Icorene 1041 YEW 2182 LLDPE combined with 2–5 wt% polyisobutylene or ULDPE tackifying blend, 0.5–1.5 wt% slip/antiblock package, and 0.5–1.0 wt% high-clarity nucleator. Winding tension is controlled at 0.1–0.3 N/mm width to prevent neck-in and roll telescoping; cling force is measured per ASTM D5458-95, tensile elongation per ISO 527-3, and puncture per ISO 7765-1:2014. Regulatory obligations include chemical registration under REACH 1907/2006; where direct food contact is not intended, EU 10/2011 migration testing is not automatically applicable but is performed when customers convert the film into indirect-contact dunnage. The terminal product is machine and hand pallet wrap in 12–30 µm thickness, including pre-stretched rolls with 200–400% stretch capacity for logistics and export packing.
In outdoor low-voltage cable jacketing, LLDPE compounds provide a lower-temperature flexibility window than plasticized PVC and are processed on single-screw extruders with 24:1–30:1 L/D barrier screws. The compound is prepared from 100 phr Icorene 1041 YEW 2182 resin, 5–20 phr of an ethylene-vinyl acetate or low-density polyethylene impact modifier, 2.5 phr furnace carbon black for ultraviolet stabilization, 0.2–0.4 phr antioxidant, and 0.05–0.10 phr processing aid. Extrusion barrel profiles are set from 130°C at the feed throat to 180–200°C at the crosshead die, with melt temperature measured per IEC 60811-401 and jacket thickness controlled from 0.8–1.4 mm. The product is cooled in a water trough at 20–40°C with line speeds of 200–600 m/min for thin-wall jackets. Compliance is evaluated under IEC 60502-1 for low-voltage insulated cables, EN 50290-2-23 for polymeric sheathing compounds, and RoHS 2011/65/EU for lead, cadmium, mercury, hexavalent chromium, and brominated flame retardant restrictions; full REACH registration under EC 1907/2006 is required for import. The main operational boundary is incompatibility of the base resin with free-radical scavenging metal deactivators in copper-cable contact: unvalidated amine-based stabilizer packages can cause premature color shift and should not be substituted without IEC 60811-401 thermal aging at 100°C/168 h. The terminal product is jacketing for outdoor low-voltage control cables, signal cables, and photovoltaic harness sheaths, where repeated flexing at −25°C without cracking is demonstrated by cold bend testing per EN 60811-504.
Competitive LyondellBasell Icorene 1041 YEW 2182 Polyethylene, Linear Low Density prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell classifies the material designated Icorene 1041 YEW 2182 as a polyethylene, linear low density resin within the Icorene polyolefin family. The 1041 base identifier is conventionally associated with rotational moulding and general-purpose low-pressure polyethylene; the YEW 2182 suffix denotes a manufacturer-specific formulation, commonly interpreted in distributor documentation as a stabilised and/or pigmented variant. The resin falls under the ISO 1872-1 designation PE-LLD because the density remains below 0.940 g/cm³. Publicly available grade summaries typically place the uncompounded Icorene 1041 base resin in a density band of 0.932–0.940 g/cm³ and a melt flow rate band of 3.0–6.0 g/10 min at 190 °C/2.16 kg; the YEW 2182 additive package can shift both values slightly. No single generic correction factor applies, and batch release certificates should be consulted for lot-specific values.
Melt flow rate and density are the most common lot-release control points. Independent distributor listings for the Icorene 1041 series frequently report density near 0.938 g/cm³ when measured according to ISO 1183-1:2019 and a melt flow rate near 5.0 g/10 min when measured according to ISO 1133-1:2022. For a stabilized and pigmented rotational moulding variant, the density may be 0.001–0.004 g/cm³ higher than the natural base resin, and melt flow rate may vary by 0.2–0.8 g/10 min depending on the masterbatch and stabilizer system.
Typical mechanical values published for linear low density polyethylene rotational moulding grades in this density range include tensile yield stress of 15–20 MPa at 50 mm/min, elongation at break of 700–900%, flexural modulus of 300–550 MPa, Shore D hardness of 55–65, and Vicat softening temperature of 110–125 °C depending on heating rate and specimen preparation. Tensile properties are frequently determined on Type IV specimens according to ASTM D638-14 Annex A3. Environmental stress crack resistance measured by ASTM D1693 Condition B in 100% Igepal frequently exceeds 500 h for linear low density polyethylene, with values above 1,000 h reported for certain Icorene 1041 lots. Low-temperature impact is not a single-point property; ductile-to-brittle transition depends on wall thickness, mould cooling rate, and internal stress distribution.
Impact assessment should be performed at part wall thickness rather than on compression-moulded plaques. In rotational moulding, cooling rate controls spherulite size; faster cooling produces smaller spherulites and higher impact resistance, but excessively fast cooling causes differential shrinkage and warpage. A cooling rate of 8–12 K/min in air before water quench yields reproducible impact retention. Published rotational moulding studies with linear low density polyethylene of comparable density show that puncture energy at -40 °C can decline by 30–50% when wall thickness increases from 4 mm to 10 mm because of plane-strain constraint.
On shuttle-type biaxial rotational moulding lines with mould lengths of 2.0–4.0 m, the grade is processed at oven temperature setpoints of 285–315 °C for wall sections in the 4–10 mm range. Peak internal air temperature is used as the release criterion; linear low density polyethylene rotational moulding powders of this class typically require a peak internal air temperature of 190–210 °C. Below 180 °C, incomplete sintering leaves pinholes and weak knit lines, particularly at corners and sharp radii. Above 220 °C, long residence accelerates thermo-oxidative chain scission; the pigmented YEW 2182 system may yellow before the unpigmented base resin. Air cooling at 6–12 K/min followed by water mist is typical; quench rates above 15 K/min can produce differential shrinkage and warpage in large flat panels.
The YEW 2182 stabilisation is intended for outdoor service. Ultraviolet stabilizer systems in polyolefins are typically hindered amine light stabilizers and ultraviolet absorbers; their concentration is not disclosed. Accelerated weathering by ISO 4892-2 with UVA-340 lamps at 0.76 W/m² irradiance can be used to compare colour fade and chalking, although part thickness and surface oxidation dominate long-term weathering. Published data for this specific configuration is limited.
Rotational moulding requires a thermoset-like powder flow and densification pattern. The grade is supplied as a ground or micro-pelletised powder. Sieve analysis is controlled by ISO 4610 or equivalent; a common top cut is 500 µm, with oversize above 500 µm held below 1.0%. Fines below 75 µm should remain below 5.0% because excessive fines increase dust, reduce apparent density, and can cause charge buildup during feeding. Apparent density by ISO 60:2023 typically falls between 0.35 and 0.45 g/cm³ for linear low density polyethylene powders of this particle architecture. Dry-flow time through a 15 mm funnel orifice measured according to ASTM D1895 is commonly 8–15 s/100 g; slower flow can indicate particle electrostatic adhesion or high fines.
On production-scale high-intensity mixers used for dry blending colour or stabilizer concentrates, impeller speeds of 300–600 rpm for 3–5 min are sufficient for uniform distribution; longer mixing at high speed generates fines and raises powder temperature. Slow tumble blending at 20–30 rpm is preferred when only a low percentage of external lubricant or pigment is added.
Rheologically, a linear low density polyethylene of melt flow rate 5 g/10 min at 190 °C typically exhibits a zero-shear viscosity in the order of 1.0–3.0 kPa·s. The melt has lower melt elasticity than a branched low density polyethylene homopolymer, which influences bubble formation and mould-surface replication during heating. Conventional Ziegler-Natta grades of this class usually have a broader molar mass distribution than single-site metallocene linear low density polyethylene, with polydispersity indices typically between 3.5 and 5.0. Metallocene grades often show a narrower distribution near 2.0–3.0. The broader distribution in the Icorene 1041 class can improve low-shear particle coalescence and mould-surface replication, while metallocene linear low density polyethylene may offer higher dart impact and better optical clarity in thin sections. Published data for this specific configuration is limited; direct tooling trials are required to quantify cycle-time difference and low-temperature impact.
The conversion from low density polyethylene homopolymer to Icorene 1041 YEW 2182 is not a drop-in substitution because the linear backbone changes melt rheology and solid-state performance. Short-chain branching in linear low density polyethylene is primarily controlled by comonomer incorporation; the linear architecture increases tie-molecule concentration relative to low density polyethylene. This produces higher slow crack resistance and higher tensile yield at comparable density, but it also reduces melt elasticity and can require additional heating to achieve complete particle coalescence. Moulding cycle time may therefore require an increment of 1–3 min or a 5–10 °C higher peak internal air temperature when switching from low density polyethylene of the same nominal melt index.
| Attribute | LDPE homopolymer | Icorene 1041 YEW 2182 class | HDPE |
|---|---|---|---|
| Density (ISO 1183-1) | 0.910–0.930 g/cm³ | 0.932–0.940 g/cm³ | 0.940–0.970 g/cm³ |
| Melt flow rate at 190 °C/2.16 kg | 2–20 g/10 min | 3–7 g/10 min | 2–10 g/10 min |
| Tensile yield stress | 8–14 MPa | 15–20 MPa | 20–30 MPa |
| Flexural modulus | 150–300 MPa | 300–550 MPa | 700–1,400 MPa |
| Environmental stress crack resistance | 10–100 h | 500–1,500 h | 20–200 h depending on comonomer |
| Low-temperature brittleness | Brittle below -20 °C | Retained to below -40 °C | Can be notch-sensitive below -10 °C |
The table above represents typical industrial performance bands, not batch release limits for a specific lot. The Icorene 1041 YEW 2182 grade occupies a distinct intermediate position: it retains more low-temperature toughness than high density polyethylene and provides higher tensile stiffness and environmental stress crack resistance than low density polyethylene homopolymer. These differences become relevant when the same tooling is used for tanks, hoppers, and thin-walled enclosures that must survive outdoor exposure and liquid contact.
The material is hydrophobic, with 24 h water absorption typically below 0.03% by ISO 62:2008; pre-drying is not normally required. If condensation has formed on cold powder, Karl Fischer titration should be used to verify moisture below 0.05 wt%; if exceeded, drying at 60–70 °C for 1–2 h in a dehumidified air drier is adequate. Storage should avoid temperatures above 40 °C and direct ultraviolet exposure to preserve the stabilizer system in YEW 2182. The base olefin polymer may be covered by 21 CFR 177.1520 or EU Regulation 10/2011 in unpigmented form, but the coloured and stabilized YEW 2182 variant requires a written compliance statement for food-contact, potable-water, or toy applications. Chemical resistance to aqueous acids and alkalis is generally high, but strong oxidising acids and certain hydrocarbon solvents will swell or degrade the surface; environmental stress cracking evaluation under ASTM D1693 or ISO 22088 should be used when creep rupture is a design concern.
| Property or control | Standard or regulation | Typical use |
|---|---|---|
| Melt mass-flow rate | ISO 1133-1:2022 / ASTM D1238 | Lot acceptance and flow classification |
| Density | ISO 1183-1:2019 | Grade classification |
| Tensile yield stress and elongation | ISO 527-2 / ASTM D638-14 | Design allowables |
| Environmental stress crack resistance | ASTM D1693 / ISO 22088 | Chemical resistance ranking |
| Instrumented puncture | ISO 6603-2 | Low-temperature impact behaviour |
| Apparent density and pourability | ISO 60:2023 / ASTM D1895 | Powder handling |
| Food-contact verification | 21 CFR 177.1520 / EU 10/2011 | Compliance confirmation |