| HS Code | 259749 |
| Polymertype | Linear Low Density Polyethylene (LLDPE) |
| Density | 0.925 g/cm³ |
| Meltmassflowrate 190c 2 16kg | 1.0 g/10 min |
| Tensilestrengthatyield | 10.3 MPa |
| Tensilestrengthatbreak | 20.7 MPa |
| Elongationatbreak | 700% |
| Flexuralmodulus | 241 MPa |
| Hardnessshored | 50 |
| Vicatsofteningtemperature | 95 °C |
| Meltingtemperature | 122 °C |
| Brittlenesstemperature | < -70 °C |
| Color | Green |
| Form | Pellets |
As an accredited LyondellBasell Icorene 1041 GRN 6619 Polyethylene, Linear Low Density factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell Icorene 1041 GRN 6619 Linear Low Density Polyethylene is supplied in 25 kg bags, palletized and shrink-wrapped for safe storage. |
| Container Loading (20′ FCL) | 20′ FCL container loading: palletized 25-kg bags of LyondellBasell Icorene 1041 GRN 6619 LLDPE, shrink-wrapped for secure, stable ocean transport. |
| Shipping | LyondellBasell Icorene 1041 GRN 6619 Polyethylene, Linear Low Density is shipped as non-hazardous solid pellets in 25 kg bags, octabins, or bulk containers. It requires no UN number, DOT/IMDG/IATA hazard class, or placards. Transport in closed, labeled containers. Keep dry, away from ignition; standard PPE recommended. Protect from UV and moisture. |
| Storage | Store in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, sparks, flames, and strong oxidizers. Keep original bags or containers closed to prevent moisture, dust, and contamination. Place on clean, dry surfaces; avoid excessive stacking or heat exposure that may cause sagging or fusing. Protect from UV light and incompatible materials. Follow local regulations and good housekeeping. |
| Shelf Life | Shelf life is 2 years when stored in a cool, dry, well-ventilated area away from direct sunlight and moisture. |
LyondellBasell Icorene 1041 GRN 6619 is supplied as a green pre-coloured linear low-density polyethylene powder for biaxial rotational moulding. The base resin belongs to the LLDPE class; general-purpose rotomoulding LLDPE grades often exhibit a density between 0.925 g/cm³ and 0.940 g/cm³ and a melt flow rate between 2 g/10 min and 7 g/10 min at 190 °C/2.16 kg as measured per ISO 1133-1:2022. Exact values for Icorene 1041 GRN 6619 must be read from the lot-specific Certificate of Analysis, because the green 6619 colour package can shift melt flow rate and thermal properties relative to the unpigmented LLDPE base. The application tracks below are evaluated for real downstream conversion operations. Where a numerical grade-specific value is not publicly available, the application description states that published data for that specific configuration are limited rather than extrapolating an unverifiable figure.
| Downstream track | Oven setpoint (°C) | Peak internal air temperature (°C) | Nominal wall thickness (mm) | Rotation ratio (major:minor) | Critical defect observed on production equipment |
|---|---|---|---|---|---|
| Agricultural tank | 280–300 | 195–205 | 8–12 | 4:1 | Corner thinning at fitting bosses |
| Marine buoyancy shell | 275–295 | 190–200 | 6–10 | 5:1 | Kiss-off voiding at rib base |
| Playground panel | 260–285 | 185–195 | 4–8 | 4:1 | Insert cold joints at bosses |
| Secondary spill pallet | 290–310 | 200–210 | 10–15 | 4:1 | Warpage on large flat floor |
| Granular hopper | 270–290 | 190–200 | 6–10 | 4:1 | Steam bubbles at rim if powder wet |
| Outdoor enclosure | 260–280 | 180–190 | 5–8 | 5:1 | Colour shift and tacky interior at high PIAT |
A vertical cylindrical fertilizer tank in the 1,000–15,000 L class is rotomoulded as a one-piece shell with integrally moulded outlet bosses, lifting lugs, and baffle pockets. The use of LyondellBasell Icorene 1041 GRN 6619 places the acceptance burden on two measurable properties: environmental stress-crack resistance under ASTM D1693 Condition B and pinhole-free shell integrity after a high-voltage spark test at 15 kV. A shot weight for a 2,000 L tank with a 10 mm nominal wall is calculated from shell surface area, the density on the Certificate of Analysis, and a powder allowance of 6–8% to compensate for thinning at the upper and lower radii and hinge-out at the pole. The mould is charged with powder that exhibits a controlled dry-flow time under ASTM D1895 Method A and a particle size distribution principally between US mesh 35 and US mesh 100. Excessive sub-100-mesh fines promote inner-surface porosity, while coarse particles above 35 mesh produce late-flow marks near the polar region. Oven setpoints of 280–300 °C and a peak internal air temperature of 195–205 °C are used for medium-wall agricultural tanks. A lower PIAT leaves unconsolidated powder at corner radii and creates micro-porosity visible at 10× magnification; a higher PIAT shifts the green shade toward yellow and raises the carbonyl index as measured by FTIR-ATR over the lot baseline. The primary-to-minor-axis rotation ratio is held near 4:1, and forced-air cooling reduces part surface temperature to 70 °C before demoulding. Liquid fertilizer formulations often contain ammonium nitrate, potassium chloride, or glycol ethers; a 30-day immersion test per ASTM D543 at 40 °C with the actual commercial dilution is required because stress-cracking is affected by the specific adjuvant package, not by generic solubility alone. Stationary tank design verification follows ASTM D1998, which addresses minimum wall thickness, head configuration, and fitting reinforcement for upright polyethylene tanks. The green powder is not a replacement for fibre-reinforced thermosets in strong oxidiser duty; continuous exposure to ≥50% sulfuric acid at elevated temperature is outside the recommended envelope. Published data for this specific grade in oxidising acid service are limited; qualification must be a field-specific protocol rather than an extrapolation from general LLDPE tables.
Buoyancy shells for floating docks and modular pontoons are rotomoulded as closed or foam-filled double-wall structures. In production, the recurring defect is not thin-wall rupture but micro-void coalescence at the base of kiss-off ribs, where two heated skins contact and transfer flexural load. The powder bed must remain mobile until the internal air reaches 190–200 °C; therefore the oven profile uses an initial heat ramp of 8–10 °C/min at the mould surface, followed by a hold plateau. Mould rotation at 5:1 major-to-minor is common for elongated floats because it avoids a thick accumulation at the end caps while maintaining coverage on the cylindrical mid-section. Nominal skin thickness is 6–10 mm, with kiss-off spacing held at roughly three times the skin thickness. Tighter spacing increases stiffness but creates localised thinning at the weld line. The green 6619 pigment package absorbs radiant heat differently from natural LLDPE; on cast-aluminium mould surfaces the surface temperature may reach the setpoint 5–10 °C earlier than an unpigmented control. This thermal offset must be confirmed with an embedded thermocouple on the mould inner wall, not inferred from oven temperature alone. After demoulding, the shell is filled with expanded polystyrene foam at a density of 12–20 kg/m³ or left as a sealed air cavity, depending on the buoyancy reserve required by the platform designer. Acceptance of the rotomoulded shell includes a low-temperature impact test per ISO 6603-2 at 0 °C or -20 °C according to service latitude, and a tensile test per ISO 527-2 on specimens cut from the flat centre of the shell. Water absorption of the LLDPE shell is negligible; however the foam core, if exposed through a crack, retains water and reduces residual buoyancy. For marine service, the outer surface is checked for micro-cracks after 1,000 h of accelerated weathering per ISO 4892-2. The green colour is not an anti-fouling system, and submerged surfaces may require a mechanical cleaning specification or a fouling-release coating after moulding. Any metal anchor insert must be isolated from the polymer with a gasket or overmoulded seal to prevent crevice corrosion at the insert shoulder.
In a rotomoulded playground tunnel or climber panel, the design loads are concentrated at handgrip bosses, hinge bosses, and connecting flanges rather than distributed hydrostatic loads. The green 6619 colour is often selected for landscape integration; however the colourant package must satisfy the migration limits of EN 71-3 for elements that could be mouthed by children, and the finished assembly must meet the structural requirements of ASTM F1487 or the relevant regional playground standard. Wall thickness is typically 4–8 mm. Thin skins shorten cycle time but reduce the thread pull-out strength of integrally moulded insert bosses. Inserts are placed on steel pins and indexed to prevent rotation during powder flow; an insert temperature below the powder sintering temperature at the moment of contact creates a cold joint around the knurl. The mould is run with a rotation ratio of 4:1 and a peak internal air temperature of 185–195 °C. Higher temperature causes a colour shift toward yellow-green and may degrade the UV stabiliser; lower temperature leaves powder speck at the internal kiss-off ribs. Because outdoor playground components experience repeated diurnal thermal expansion, the converter should conduct a cyclic thermal test between -20 °C and 60 °C for 100 cycles and inspect for surface cracks at the fastening points. Impact testing is performed on prototype parts per ISO 6603-2 at -20 °C, with ductile puncture preferred over brittle cracking. Surface colour and gloss are measured after 1,000 h of xenon arc exposure per ISO 4892-2; acceptance is typically a maximum ΔE of 3.0 against an unexposed reference, but the exact ΔE target must be set by the buyer because grade-specific colour ageing data are not always published. Adhesive bonding of EPDM seals to the LLDPE surface is difficult; mechanical joining or hot-plate welding is preferred for multi-part assemblies. Published data for this specific grade in playground load cases are limited; therefore first-article testing on a production-representative part is mandatory.
| Downstream track | Governing standard or regulation | Critical test method | Acceptance measure | Operational boundary |
|---|---|---|---|---|
| Agricultural tank | ASTM D1998 | ASTM D1693 Cond B, ASTM D543 | No pinholes after spark test; no stress-cracking after chemical immersion | Not for strong oxidisers at elevated temperature |
| Marine buoyancy shell | ISO 6603-2 | ISO 6603-2, ISO 527-2 | Ductile puncture at service temperature; tensile values meet design | Foam core retains water if shell cracks |
| Playground panel | EN 71-3, ASTM F1487 | EN 71-3, ISO 6603-2 | No migration limit exceedance; ductile failure at -20 °C | Colourant must be cleared for child contact |
| Secondary spill pallet | 40 CFR 112.7, applicable fire code | ASTM D543, ASTM D638 | Containment volume per jurisdiction; sufficient retained elongation | Hydrocarbons and oxidising acids may require liner |
| Granular hopper | FDA 21 CFR 177.1520 | ASTM D4060, IEC 61340-2-3 | Food-contact clearance for finished article; application-specific abrasion loss | Continuous service above 50 °C not recommended |
| Outdoor enclosure | IEC 60529 | ISO 6603-2, IEC 60529 | IP rating; lid seat flatness 0.5 mm | Water-quench cooling weakens low-temperature ductility |
A secondary spill pallet for 200 L drums is a thick-walled rotomoulded tray with a sump capacity governed by 40 CFR 112.7 or the applicable national fire code. The containment volume must be sized according to the jurisdiction’s formula for the largest single container or an aggregate percentage of stored liquids; designing to the more conservative of the two values is the standard production practice. The raised deck must support static load without creep rupture. The Icorene grade is processed as a medium- to thick-wall shell of 10–15 mm, with internal pillars or cored ribs moulded as one piece to carry the drum load. The oven setpoint is 290–310 °C, and the PIAT is held between 200 °C and 210 °C because thicker walls require a longer internal plateau to eliminate a cold core. Premature demoulding produces a frozen-in thermal gradient; the part then develops a concave bow across the large flat sump floor. Post-mould dimensional inspection uses a granite surface plate and feeler gauges; bow of more than 3 mm over 1 m is typically rejected for pallets that must stack. Chemical resistance is validated by immersion of cut coupons in the stored liquids at 40 °C for 30 days per ASTM D543, followed by tensile testing per ASTM D638 to measure retained elongation at break. Stress-crack resistance under ASTM D1693 Condition C is more relevant than Condition B for thick sections because residual stress from non-uniform cooling is higher. The green colour must remain legible as a safety boundary; UV exposure per ISO 4892-2 for 1,000 h should not reduce contrast against the floor marking below the site’s safety sign standard. Operational boundaries include incompatibility with concentrated oxidising acids and with hydrocarbons that plasticise the LLDPE matrix; a liner or alternative polymer is required for such service.
Where dry granular products discharge through a rotomoulded hopper, the inner wall must resist sliding abrasion while maintaining sufficient thermal conductivity during moulding to prevent cold spots at the outlet flange. LyondellBasell Icorene 1041 GRN 6619 is suitable for hoppers and bins that are not subject to continuous elevated temperature above 50 °C, because LLDPE softens and unsupported sidewalls can creep under column load. The nominal wall thickness is 6–10 mm, with corner radii kept above 12 mm to reduce stress concentration at the transition from cone to cylinder. Outlet flanges are rotomoulded as a thickened rim and then machined flat to prevent granular leakage at the seal face. The mould is run at an oven setpoint of 270–290 °C and a PIAT of 190–200 °C; the powder moisture content before charge should be below 0.05% by weight, because steam generated during the heat cycle causes surface bubbles and weakens the rim. Abrasion resistance is measured by the weight loss of a disc specimen under ASTM D4060 Taber abrasion with an H-18 wheel and 1,000 g load; the numerical acceptance is application-specific. For food-contact ingredients, compliance with FDA 21 CFR 177.1520 must be demonstrated on the finished article, including the colourant package. The base LLDPE may meet the appropriate extractives limit, but the green 6619 pigment and any processing aids must be cleared for the intended food type and temperature. If no food-contact clearance letter is available for the pigmented grade, the bin is limited to non-food contact or must be lined. Static electricity build-up is possible during discharge of fine powders; the surface resistivity of natural LLDPE is modified by the green pigment, so a charge decay test per IEC 61340-2-3 should be performed before the bin is used in a combustible dust environment.
Enclosures for irrigation valves, underground sensor nodes, and landscape electrical junctions require impact resistance at sub-zero temperatures and sufficient dimensional stability to keep the cover seated. The green 6619 colour is beneficial for visual identification in landscaped areas, but the UV resistance of the package must be separated from the natural LLDPE’s inherent low-temperature ductility. The shell is rotomoulded at 5–8 mm thickness; the mould may be run with a lower oven setpoint of 260–280 °C because thinner walls reach the PIAT plateau faster. Peak internal air temperature remains 180–190 °C; exceeding 200 °C on a thin-wall enclosure can shift the green hue and produce a tacky interior surface if the stabiliser package is exhausted. Ductility at -20 °C is checked by a multi-axial impact test per ISO 6603-2 on flat specimens cut from the lid. A brittle failure indicates inadequate sintering or frozen-in stress from rapid cooling. Rapid water-quench cooling, which improves cycle time, should be avoided because it increases residual stress at the gasket seat and reduces low-temperature impact margin. The cover seat is post-machined to maintain flatness within 0.5 mm over the opening; a bowed seat breaks the gasket line and allows ingress of soil water. Published data for this specific grade in buried enclosure service are limited; the qualification plan should therefore include a 500 h multiple-temperature cycling test between -30 °C and 70 °C with the enclosure assembled and sealed, followed by an ingress protection test per IEC 60529 at the specified IP rating.
Competitive LyondellBasell Icorene 1041 GRN 6619 Polyethylene, Linear Low Density prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 1041 GRN 6619 is a linear low-density polyethylene rotational molding grade supplied as a pre-colored green powder. The numerical grade 1041 identifies the melt-flow and density position within the Icorene rotomolding portfolio, while GRN 6619 specifies the green colorant formulation incorporated into the powder. Under ASTM D883, linear low-density polyethylene comprises ethylene copolymers with a density range of 0.915–0.940 g/cm³; the measured density of the pre-colored configuration may shift slightly within or above this range because of pigment and dispersion aids. The product is intended for monolayer rotational molding of hollow parts requiring a balance of low-temperature impact resistance, environmental stress-crack resistance, and moderate stiffness. The pre-colored supply form removes dry-blending of color concentrate at the molding shop, reducing let-down error and improving color consistency.
All release specifications for Icorene 1041 GRN 6619 must be read from the manufacturer’s certificate of analysis and technical data sheet. Published data for this specific pre-colored configuration are limited in public compilations; the base LLDPE resin is characteristically tested for melt flow rate under ASTM D1238-20 Procedure A at 190 °C and 2.16 kg, and for density under ASTM D1505. The green pigment concentrate can alter the measured melt flow rate and density relative to the natural base resin, so natural-grade values cannot be assumed to apply exactly to GRN 6619 without verification.
The linear low-density polyethylene structure consists of a predominantly linear backbone with controlled short-chain branching introduced by low-pressure copolymerization. This architecture differs from high-pressure low-density polyethylene, which contains long-chain branching, and from high-density polyethylene, which contains minimal short-chain branching. In rotational molding, the short-chain branches in LLDPE produce a combination of lower flexural modulus than HDPE, higher tensile strength and puncture resistance than LDPE, and environmental stress-crack resistance superior to many conventional HDPE rotomolding grades. The density-controlled branching also influences sintering kinetics: LLDPE powders of this class form a densified melt layer at lower internal air temperature than HDPE, but they require more attention to cooling rate if part warpage and shrinkage must be controlled.
The distinction is not solely compositional. Rotational molding grades of LLDPE are ground to a specific particle-size distribution and stabilized for repeated oven dwell, whereas injection-molding LLDPE grades with higher melt flow may not tolerate the long residence times typical of rotomolding. Icorene 1041 GRN 6619 is positioned for rotational molding rather than high-shear extrusion because its molecular architecture and additive package are selected for zero-shear sintering, bubble release, and wall densification in a rotating mold. Direct substitution of an injection-molding LLDPE would introduce viscosity differences, pigment dispersion issues, and possible oxidative instability at rotomolding oven temperatures.
Specification verification for this material class depends on standard tests that correlate with rotomolding performance rather than with high-shear processing behavior. The following table identifies the test methods commonly used for release testing and incoming inspection of LLDPE rotomolding powders.
| Attribute | Standard method | Rotomolding relevance |
|---|---|---|
| Melt flow rate | ASTM D1238-20 Procedure A, ISO 1133-1:2022 at 190 °C/2.16 kg | Indicates melt viscosity and bubble-release behavior; excessive melt flow can reduce melt strength and increase pinhole risk. |
| Density | ASTM D1505, ISO 1183-1:2019 | Controls stiffness, permeability, and part weight; pigment loading may shift measured density. |
| Flexural modulus | ASTM D790-17, ISO 178:2019 | Predicts short-term load-bearing deflection in large hollow parts. |
| Tensile yield stress and elongation | ASTM D638-14, ISO 527-2 | Provides design data for wall sections and post-mold joining. |
| Environmental stress-crack resistance | ASTM D1693-15 | Assesses resistance to slow crack growth under surfactant exposure. |
| Low-temperature impact | ISO 6603-2, ARM low-temperature impact test | Evaluates brittle-ductile transition in cold-service rotomolded parts. |
Rotational molding of a pre-colored green LLDPE powder is governed by oven dwell temperature, internal mold air temperature, and cooling rate. The green colorant alters infrared absorption compared with natural translucent powder, so oven set points may be reduced or dwell shortened to avoid surface oxidation. General LLDPE rotomolding practice uses an internal air temperature between 190 °C and 210 °C and an oven temperature between 280 °C and 320 °C, depending on part wall thickness, oven type, and mold gauge. These values are class-typical processing conditions; the Icorene 1041 GRN 6619 technical data sheet may identify a narrower window for the specific pigment and stabilization package.
During oven dwell, the powder bed tumbling against the mold surface sinters into a porous melt layer that progressively densifies as the wall temperature rises. In a multi-axis rotational molding machine, wall thickness uniformity depends on maintaining the mold rotation ratio and ensuring that the powder does not bridge in deep ribs or narrow undercuts. The internal air temperature should be monitored with an infrared pyrometer or thermocouple feedthrough because the mold surface temperature alone does not indicate whether the inner wall has reached complete melt densification. Extended exposure beyond 220 °C internal air can initiate oxidative degradation, leading to discoloration, carbonyl formation, and a loss of impact performance.
Cooling rate after oven dwell controls crystallinity and shrinkage. Fast cooling by water spray or forced air increases nucleation and produces smaller spherulites, which generally improves impact toughness but increases residual stress and warpage risk. Slow ambient cooling allows higher crystallinity, greater stiffness, and higher shrinkage. For large rotomolded parts produced from green LLDPE, the cooling step should be staged so that the inner wall cools while the part is still supported by the mold to minimize sink marks and dimensional drift. A premature demolding at high wall temperature can produce distortion at the gate, parting line, or flat panel sections because the low thermal conductivity of polyethylene retains heat in the inner wall.
Because the material is a pre-colored powder, storage conditions before molding also affect processing. The powder is not hygroscopic in the sense of requiring desiccant drying, but condensation on cold powder surfaces can introduce moisture that forms pinholes during bubble escape. When powder stored at low temperature is transferred into a warm molding room at relative humidity above 60%, surface condensation is possible. Sealed original containers should be allowed to equilibrate to the molding area before opening, and partially used containers should be closed immediately to avoid dust, ambient moisture, and contamination.
Outdoor weathering of GRN 6619 green rotomolded parts depends on the pigment system and the ultraviolet stabilization package supplied in the grade. Green pigments can vary in their UV screening behavior and heat build-up. Color alone does not prevent polymer chain scission; stabilizers are required for continuous outdoor service. Weathering performance is commonly screened by ASTM G154 fluorescent UV exposure or ISO 4892-2 xenon arc exposure, with color change measured by ASTM D2244 or ISO 7724-3. Surface chalking and gloss loss can occur before bulk mechanical failure, so specifications for outdoor applications should include both color retention and retained tensile or impact properties after accelerated exposure.
Rotomolded parts made from Icorene 1041 GRN 6619 are often assembled by hot-plate welding, butt fusion welding, or mechanical fastening. Weld integrity is dominated by surface oxidation, contamination, and the crystallinity profile left by the rotomolding cycle. Because polyethylene has low surface polarity, adhesive bonding requires surface activation by flame, corona, or plasma treatment; untreated surfaces generally fail in low-energy adhesion. For structural hot-gas or extrusion welding, the oxidized outer skin must be removed by scraping immediately before welding to expose unoxidized polymer. Molded-in stress from rapid cooling can distort the weld zone, so parts should be fixtured during joining and allowed to stabilize after demolding.
The cooling rate used in the rotomolding cycle affects weld quality because it alters spherulite size and crystalline orientation. A fast-cooled wall may exhibit lower crystallinity and higher toughness but can contain residual thermal stress that relaxes during welding. A slow-cooled wall may have higher modulus and higher crystallinity but can be more susceptible to brittle fracture at the weld root. Processors should evaluate weld tensile strength using ASTM D638-14 Type IV specimens machined from welded plaques or assemblies. Acceptable weld factors depend on part geometry and service load; published data for this specific pre-colored product configuration are limited, so lot-specific qualification is required for load-bearing welded structures.
Rotational molding powder performance begins with particle-size distribution and dry-flow character. The powder should pack uniformly against the mold surface and sinter without entrapping air. A typical LLDPE rotomolding powder is ground to pass 35 mesh (500 µm) with a controlled level of fines below 200 µm because excessive fines can create airborne dust in the mold cavity and cause uneven wall thickness. Coarse particles sinter more slowly and can leave pinholed or uneven inner surfaces. The exact particle-size curve for Icorene 1041 GRN 6619 should be confirmed on the certificate of analysis because pre-colored grinding and blending can shift the distribution relative to natural powder.
Dry-flow time is measured by funnel methods such as ASTM D1895 or an equivalent rotational molding powder flow test. A dry-flow value that is too high indicates poor powder flow into narrow sections and ribs, while a very low value may indicate excessive fines or poor particle packing. Lot-to-lot variations in powder flow can produce wall-thickness differences even when the same rotomolding cycle is used. Therefore, incoming inspection should include dry-flow testing and a screen analysis rather than relying only on melt flow rate and density. Consistent powder quality reduces the need to adjust oven dwell and rotation parameters from lot to lot.
The material differences between Icorene 1041 GRN 6619 and alternative rotomolding resins are summarized through the structural and density contrasts that control stiffness, impact, and chemical resistance.
| Material class | Density range | Branching architecture | Rotomolding consequence |
|---|---|---|---|
| Linear low-density polyethylene | 0.915–0.940 g/cm³ | Linear backbone with controlled short-chain branches | Higher ESCR and low-temperature impact than HDPE, lower flexural modulus than HDPE. |
| High-density polyethylene | 0.941–0.965 g/cm³ | Minimal short-chain branching | Higher stiffness and heat deflection but lower ESCR and cold-impact resistance. |
| Low-density polyethylene | 0.910–0.925 g/cm³ | Long-chain branching from high-pressure polymerization | Easier sintering but lower tensile strength, lower stiffness, and lower puncture resistance. |
For food-contact, potable water, or toy applications, the compliance status of the pre-colored product is not automatically identical to the natural base resin. The base LLDPE may be manufactured to support 21 CFR 177.1520 for olefin polymers, while the green colorant in GRN 6619 must be separately evaluated under the applicable colorant regulation or food contact substance notification. Industrial articles sold in the European Union may require REACH registration documentation and conformity to RoHS Directive 2011/65/EU, especially for pigment metal content. Regulatory compliance statements should be requested from LyondellBasell for the exact grade and color code before use in regulated applications.
Incoming resin handling should exclude contamination with polypropylene, silicone mold release, or incompatible colorants because even minor contamination can produce localized delamination, pinhole clusters, or surface defects in thin-walled rotomolded parts. Silicone release agents can migrate into the melt surface and interfere with post-mold welding or coating. If release agents are required for complex tooling, use a grade recommended for polyolefin rotomolding and verify adhesion after molding. The operational boundary for this material is defined by the manufacturer’s grinding specification, stabilization package, and rotomolding window; use outside that boundary requires trial qualification because published data for this specific pre-colored configuration are limited.