| Density | 0.955 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 0.35 g/10 min |
| Tensile Modulus | 1250 MPa |
| Tensile Stress At Yield | 27 MPa |
| Tensile Strain At Break | >600% |
| Charpy Notched Impact Strength At 23 C | 15 kJ/m² |
| Charpy Notched Impact Strength At 30 C | 5 kJ/m² |
| Vicat Softening Temperature | 128 °C |
| Melting Point | 133 °C |
| Hardness Shore D | 65 |
| Escr 10 Igepal F50 | >1000 h |
| Water Absorption | <0.01% |
| Thermal Conductivity | 0.38 W/mK |
| Coefficient Of Linear Thermal Expansion | 1.5E-4 /°C |
As an accredited LyondellBasell HDPE H5623X01 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell HDPE H5623X01 is typically packaged in 25 kg polyethylene bags, 40 bags per pallet, 1,000 kg net. |
| Container Loading (20′ FCL) | Container loading description: LyondellBasell HDPE H5623X01 high-density polyethylene resin, supplied in 25 kg bags, loaded into a 20-foot FCL container. |
| Shipping | LyondellBasell HDPE H5623X01 is a non-hazardous, pelletized high-density polyethylene. It is shipped in 25 kg bags, octabins, bulk trucks, or railcars. Transport as non-dangerous goods with no UN number. Store cool, dry, and clean, away from sunlight, moisture, and contamination; avoid excessive heat and static ignition. |
| Storage | Store LyondellBasell HDPE H5623X01 in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, ignition sources, and strong oxidizers. Keep original bags or containers closed, clean, and off the ground to prevent moisture and contamination. Avoid prolonged outdoor storage and excessive stacking. Follow supplier SDS/local regulations for safe handling. Maintain FIFO inventory. |
| Shelf Life | LyondellBasell HDPE H5623X01 has a typical shelf life of 24 months when stored unopened, cool, dry, away from sunlight and moisture. |
Open-head industrial pails with capacities between 10 L and 25 L are a primary injection-moulded packaging application for LyondellBasell HDPE H5623X01. Datasheet values for density at 0.956 g/cm³ per ISO 1183-1 and melt flow rate at 2.3 g/10 min per ISO 1133-1 under 190°C/2.16 kg support filling of thick-walled pail bodies with nominal wall sections from 2.2 mm to 4.0 mm. A 20 L open-head pail typically requires a shot mass of 1.2–1.6 kg; the injection unit is specified with shot capacity at least 20% above part mass so that melt cushion remains between 3 mm and 8 mm. Barrel temperatures are profiled from 180°C in the feed zone to 220–240°C in the metering zone, with the nozzle held at 215–235°C. Screw configuration for pail moulding favours a compression ratio of 2.8:1 to 3.2:1, L/D ratio of 20:1 to 24:1, and a pin-type mixing section of 6–8 rows. Injection fill time is profiled so that the flow front reaches the lip ring in 0.8–1.2 s; switch-over occurs at 95–98% of cushion volume, followed by holding pressure of 30–50 MPa until gate freeze. Core cooling water is set to 10–20°C and cavity water to 8–18°C. Clamp force for a single-cavity pail tool is generally 500–800 tonnes, with total cycle time of 35–50 s depending on lip-ring thickness and demoulding temperature. A process boundary appears when part ejection is attempted above 80°C surface temperature: lip ovality can exceed 3 mm and must be corrected with post-mould cooling fixtures holding the pail for 45–90 s.
Dangerous-goods pails are qualified under UN 1A2/Y packaging requirements. Drop testing follows 49 CFR 178.603; filled pails conditioned at −18°C are dropped from 1.2 m for packing group II when the filled-density product does not exceed 1.2 g/cm³. Stack testing follows 49 CFR 178.606, applying the equivalent load of a 3 m stack of filled containers for 28 days at 40°C. Formulation ratios are kept within defined limits: colour masterbatch at 1.0–2.5 wt%, UV stabilizer masterbatch at 0.3–0.8 wt% for outdoor storage, and clean in-house regrind at 15–30 wt%. Regrind above 30 wt% is constrained by notched impact loss and visible flow lines at the sidewall-to-bottom transition when pigment dispersion is poor. The terminal article is an integrally coloured open-head pail with gasketed lid seat, used for water-based emulsions, lubricant additives, and industrial cleaning compounds.
Closure moulding shifts the control variable from part mass to gate-to-gate balance. In a 32- or 48-cavity hot-runner tool producing 0.8–2.8 g HDPE closures, shot-to-shot mass deviation is maintained below 0.5% by holding melt cushion at 3–6 mm and applying decompression of 8–12 mm after plastication. Barrel temperatures are profiled from 170°C in the feed zone to 210–230°C at the nozzle; mould cooling water is set to 10–15°C. Cavity pressure at transfer is 25–45 MPa. Cycle time for a 0.8 g tamper-evident band closure can run 5.5–7.5 s; a thicker linered cap with wall thickness 1.2–1.6 mm for UHT dairy packs extends to 9–12 s. Formulation ratios include white titanium dioxide masterbatch at 0.6–1.2 wt% and slip/antiblock masterbatch at 0.1–0.3 wt% only when top-load removal torque on a 28 mm PCO 1881 finish exceeds 1.0 N·m. Compliance for food-contact closures references FDA 21 CFR 177.1520; EU migration testing under EU 10/2011 uses overall migration limits of 10 mg/dm² in food simulants assigned by contact type. For dairy closures, sensory evaluation by DIN 10955 at 40°C for 10 days is added when taste or odour transfer is a release criterion. Torque retention after application is measured by ASTM D2063. Throughput of 32 cavities at 6 s cycle consumes approximately 16–20 kg/h; if hopper residence time exceeds 45 min at 230°C, melt discolouration begins at hot-runner drops, and valve-gate tips should be purged with high-viscosity HDPE before restart.
Ventilated distribution crates of 600×400 mm footprint are moulded from HDPE H5623X01 at shot weights of 1.6–2.9 kg depending on rib density and base design. Filling of rib sections with nominal wall thickness from 1.2 mm to 2.0 mm requires melt temperature of 230–250°C and injection speed of 40–70 mm/s. Flow-length-to-wall-thickness ratios above 350:1 in rib corners are sensitive to gate freeze-off; gate diameter is therefore held at 2.5–3.5 mm, and packing pressure is ramped from 45 MPa down to 20 MPa over 3.0–5.0 s. Clamp force calculations for a two-cavity crate tool assume 0.45–0.65 tonnes/cm² of projected area. Tools with 1,200–1,500 cm² per cavity are run on 500–700 tonne machines. Two-circuit mould temperature control is standard: cavity temperature at 12–18°C, core at 8–14°C. Melt-flow index shift after processing is recorded; an increase above 10% relative to virgin indicates molecular weight reduction from excessive shear in hot-runner channels. Regrind from post-industrial crate scrap is added at 20–50 wt%. At 50 wt% regrind, flexural modulus measured by ISO 178 falls to 1,000–1,100 MPa, which remains acceptable for closed-loop retail logistics but below typical specifications for high-stack agricultural crates. Drop testing is performed under ISO 2248. Compliance includes EU 94/62/EC packaging heavy-metal limits, where the sum of lead, cadmium, mercury and hexavalent chromium is below 100 mg/kg, and REACH Article 33 communication when any SVHC exceeds 0.1 wt%. Terminal products are returnable crates, pallet boxes, and distribution trays with moulded-in barcode pads.
Thin-wall dairy tubs and lids of 0.8–1.2 mm nominal wall are produced in stack moulds with 4+4 or 6+6 cavity configurations. Machine selection follows screw recovery rather than clamp force because projected-area-to-shot-volume ratio is high. At 1.1 mm wall, a 500 g tub and lid set is injected at 80–120 mm/s screw speed with melt temperature of 200–220°C. Cooling time is set at 3.5–6.0 s; ejection is enabled when core-side surface temperature is below 70°C. High-speed filling creates shear heating of 8–15°C across the runner, so nozzle temperature is offset −10°C from the melt set-point to avoid surface splay in the tub base. Masterbatch letdown is 0.8–1.5 wt%; titanium dioxide levels above 3.0 wt% generate melt-pressure rises of 8–15% and require screw back pressure reduction from 0.8 MPa to 0.5 MPa to prevent vent flow. Food-contact compliance includes EU 10/2011, FDA 21 CFR 177.1520, and China GB 4806.7-2016; organoleptic transfer is tested by DIN 10955 at 40°C for 10 days. Tear strength of the lid nubbin is validated on specimens cut from the hinge area using ASTM D638 Type IV. The terminal product is a dairy or margarine tub with snap-on lid, where the hinge must survive 20 opening cycles without stress whitening. Pre-drying is not required when polymer is stored in closed silos below 60% relative humidity; if pellet surface moisture exceeds 0.05 wt%, splay appears and the material must be dried at 80°C for 2 h.
Measuring chambers and overcap shells for agrochemical products require chemical resistance to dilute hydrocarbons, ester solvents, and oxidizer-based disinfectants. H5623X01 is used for injection-moulded measuring chambers and overcap shells with wall thickness from 1.8 mm to 3.5 mm. Melt temperature is set at 220–240°C and cycle time is extended to 18–30 s to permit adequate crystallinity and keep post-mould shrinkage below 1.5%. Dimensional stability after 48 h at 50°C in contact with 5% sodium hypochlorite is assessed by measuring thread diameter change; maximum acceptable increase is 0.35 mm on a 45 mm neck finish. Compliance for crop-protection packaging may include UN marking for limited quantity or full dangerous goods depending on formulation. Stress-cracking resistance is screened by ASTM D1693 Condition B in 10% Igepal CO-630 at 50°C. Antioxidant masterbatch is added at 0.2–0.5 wt% when product contact involves metal ion contamination above 1 ppm, particularly copper from pump parts. Published data for long-term ESCR of H5623X01 in ester-based agricultural emulsions is limited; pilot trials with the final formulation are required before conversion from fluorinated HDPE or PA barrier structures. Moulded-in threads with 0.8 mm root radius may crack if ejection is forced before 10 s cooling; 1.2–1.5 mm root radii are used for oxidizer-contact parts. The terminal products are graduated dosing cups, overcap shells, and secondary thread adapters for crop-protection and industrial disinfectant packs.
| Application | Melt temperature | Mould temperature | Compliance anchor | Process boundary |
|---|---|---|---|---|
| Open-head industrial pails | 210–240°C | 8–20°C | 49 CFR 178.603, 49 CFR 178.606 | Ejection below 80°C to limit lip ovality |
| Multi-cavity closures | 210–230°C | 10–15°C | EU 10/2011, 21 CFR 177.1520 | Residence time below 45 min at nozzle |
| Returnable logistics crates | 230–250°C | 8–18°C | EU 94/62/EC, REACH Article 33 | Regrind limited to 50 wt% |
| Thin-wall dairy tubs and lids | 200–220°C | 8–20°C | EU 10/2011, GB 4806.7-2016 | Pellet moisture below 0.05 wt% |
| Agrochemical measuring chambers | 220–240°C | 10–25°C | ASTM D1693, UN packaging | Thread root radius ≥1.2 mm |
Competitive LyondellBasell HDPE H5623X01 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell HDPE H5623X01 is a high-density polyethylene injection molding resin supplied in natural pellet form. Manufacturer-published nominal values include a melt mass-flow rate of 23 g/10 min tested at 190°C under a 2.16 kg load according to ISO 1133-1:2022 and a density of 0.956 g/cm³ according to ISO 1183-1:2019. The grade belongs to the high-flow segment of the Hostalen HDPE portfolio and is characterized by a linear, narrow-molecular-weight-distribution structure intended to balance injection-molding productivity with stiffness and dimensional repeatability. In production-scale equipment, the resin has been processed on hydraulic and electric injection molding machines with screw diameters from 35 mm to 60 mm and thermoplastic check-ring assemblies; published data for specific machine configurations is limited to manufacturer technical service documentation.
Compliance status for food-contact use is formulation- and lot-dependent. The grade may be evaluated under EU Regulation 10/2011 for plastics intended to contact food; however, converters are responsible for verifying overall migration and specific migration limits under final part conditions. The resin itself is not compounded with slip or antistatic additives unless specified by the supplier; therefore, coefficient of friction and static dissipation properties must be adjusted through masterbatch additions validated to ISO 8295 and IEC 61340-2-3 as applicable.
Melt viscosity is the primary material variable governing injection pressure. The 23 g/10 min melt mass-flow rate corresponds to a low-viscosity HDPE relative to grades in the 1 g/10 min to 8 g/10 min range typically used for blow molding or thick-wall industrial containers. Capillary rheometry at 190°C to 230°C shows that HDPE viscosity decreases with shear rate in a non-Newtonian manner typical of linear polyethylene; however, the standard datasheet does not include Cross or Carreau model coefficients, so Moldflow simulations should be fed with measured viscosity curves. The high melt flow rate reduces pressure drop in the sprue, runner, and gate, but the flow length is also controlled by the ability of the mold to vent. Inadequate venting at the end of fill causes compression and limits filling more than material viscosity. Pressure transducers placed near the gate have recorded peak cavity pressures below 70 MPa at melt temperature 220°C and filling time 0.4 s in laboratory thin-wall tools; transfer to production stack molds requires confirmation via short-shot series because hot-runner manifold imbalance can add 10 MPa to 20 MPa to the required setpoint. Specific pressure limits for any tool should be derived from in-mold sensors rather than from material data sheets alone.
Nominal tensile properties of HDPE H5623X01 include a yield stress near 26 MPa and a tensile modulus near 1100 MPa when tested according to ISO 527-2 at 23°C. Elongation at yield is typically below 10%. Notched Charpy impact strength is approximately 2.5 kJ/m² at 23°C and approximately 1.5 kJ/m² at -30°C under ISO 179-1/1eA. The Vicat softening temperature under ISO 306 Method A50 is approximately 127°C. Flexural modulus is frequently reported in the range 1050 MPa to 1200 MPa under ISO 178. The property set places H5623X01 among stiff HDPE grades; however, the notched impact value indicates that the grade is less damage-tolerant than low-flow HDPE grades. For living-hinge structures or snap-fit closures, the flexural modulus supports closure spring-back, but repeated flexural loading should be validated by component testing because standard single-point mechanical properties do not predict fatigue crack initiation under cyclic loading.
| Property | Test standard | Nominal value | Unit |
|---|---|---|---|
| Melt mass-flow rate | ISO 1133-1:2022 | 23 | g/10 min |
| Density | ISO 1183-1:2019 | 0.956 | g/cm³ |
| Tensile yield stress | ISO 527-2 | 26 | MPa |
| Tensile modulus | ISO 527-2 | 1100 | MPa |
| Charpy notched impact at 23°C | ISO 179-1/1eA | 2.5 | kJ/m² |
| Charpy notched impact at -30°C | ISO 179-1/1eA | 1.5 | kJ/m² |
| Vicat softening temperature A50 | ISO 306 | 127 | °C |
Pre-drying is not normally required for HDPE H5623X01 when resin is stored in sealed containers and relative humidity remains below 60%. Surface condensation on cold pellets transferred into a warm manufacturing environment can cause splay or silver streaks. Hopper dryers set at 60°C to 80°C for 2 h remove surface moisture without altering the polymer. The melt temperature window is 180°C to 280°C; thin-wall closure tools typically operate between 200°C and 240°C to reduce melt-pressure loss while avoiding visible degradation. Mold temperature is typically held at 20°C to 60°C. Lower mold temperatures shorten cooling time but increase in-mold stress and can degrade part flatness. Back pressure is normally maintained below 1.5 MPa because higher back pressure increases screw-recovery torque and viscous heating, producing melt-temperature swings that alter fill time in screw-recovery-limited cycles. Injection velocity should be set to fill the cavity as quickly as the venting system permits; excessive velocity causes jetting in thick sections, while insufficient velocity produces premature freeze-off in thin sections.
| Processing variable | Reference range | Unit | Equipment type |
|---|---|---|---|
| Melt temperature | 180–280 | °C | injection molding machine, screw diameter 35–60 mm |
| Mold temperature | 20–60 | °C | water-cooled tooling |
| Back pressure | 0–1.5 | MPa | hydraulic or electric injection unit |
| Pre-drying temperature | 60–80 | °C | hopper dryer |
| Pre-drying time | 2 | h | hopper dryer |
In cap and closure applications, the combined demands of thread dimensional tolerance, seal-surface flatness, and environmental stress crack resistance are often more restrictive than short-term tensile properties. Mold shrinkage of HDPE H5623X01 is influenced by wall thickness, gate design, packing pressure, and mold temperature; values in the range 1.2% to 2.5% are representative for injection-molded HDPE of this density class under ISO 294-4 conditioning. Closure roundness is highly sensitive to cooling asymmetry. A mold temperature difference of 5°C between cavity sides can produce out-of-roundness in thin-wall closures, particularly when a hot-runner system delivers melt at different temperatures across drops. The grade’s ESCR performance under ASTM D1693 is typically below that of medium-density and low-flow HDPE grades; the high flow and relatively high density reduce the capacity for slow energy dissipation in the presence of stress-cracking fluids such as detergents, surfactants, and some oil-based formulations. For aggressive product contact, cap liners or barrier layers are frequently required. Published data for specific closure geometries under application torque and liner compression is limited, so seal-performance validation must be performed on production tooling with the intended closure design.
Substitution of a low-flow HDPE with H5623X01 in existing thin-wall injection molds changes several processing responses at once. Filling pressure and clamp force requirements decrease at equivalent melt temperature because the higher melt mass-flow rate lowers viscosity; however, the lower melt strength increases the tendency for gate-stringing in open-nozzle systems and reduces the stability of large parison-like melt fronts. The narrower molecular weight distribution reduces post-filling warpage from anisotropic stress relaxation, but it also reduces notched impact toughness and ESCR compared with HDPE grades having melt flow rates below 1 g/10 min. In cap and closure tools originally designed for medium-flow HDPE, the material may permit faster filling and shorter packing time; however, actual cycle-time reduction is cooling-limited and must be confirmed by dimensional capability studies. The grade is not a direct substitute for blow-molded bottles, canisters, or large industrial containers where long-term hoop stress and slow crack growth resistance are primary design parameters. Machine settings should be re-established by short-shot series starting at 200°C barrel temperature and increasing to 240°C as needed; mold temperature should be controlled at 30°C to 50°C for uniform shrinkage and roundness.
In high-density polyethylene injection molding, the temperature rise from viscous dissipation in small gates and hot-runner drops can exceed 20°C under high injection velocities. For H5623X01, this shear heating lowers local melt viscosity and aids filling; however, it can also create variability in melt temperature between cavities if hot-runner manifold balance is imperfect. The grade’s high flow accentuates the sensitivity of fill time to melt temperature changes because a temperature increase from 200°C to 220°C reduces viscosity enough to shift the filling pattern in multi-cavity tools. Molding trials on tools with 8 or more cavities should therefore include thermal imaging or melt-temperature sensors at the nozzle tips rather than relying solely on barrel setpoints. Gate diameters below 0.8 mm may generate excessive shear rates and can cause local molecular orientation or surface streaking; the use of needle shut-off hot tips with optimized valve timing is common in closure tooling to control gate-stringing and improve gate-vestige consistency.
Regrind of HDPE H5623X01 can be reused in injection molding at levels up to 30 wt% without loss of melt stability in most thin-wall tools, provided the regrind is dry, free of oil contamination, and uniformly blended. Higher regrind levels reduce melt flow consistency because of molecular weight reduction and contamination with degraded polymer from previous heat histories. The exact regrind limit depends on the thermal history of the scrap and the acceptable part dimensional capability. For food-contact articles, recycled content may be prohibited or restricted under EU Regulation 10/2011 and 21 CFR 177.1520 unless the recyclate is produced under a specific authorization or behind a functional barrier. No statement on this webpage substitutes for lot-specific compliance certificates.
Rheological data for Moldflow simulation should be generated using capillary and cone-plate rheometry across 0.1 s⁻¹ to 10,000 s⁻¹ and 180°C to 280°C. The standard datasheet of HDPE H5623X01 does not provide Cross-WLF constants; therefore, simulation users must input measured viscosity curves and pressure-specific volume-temperature data for reliable prediction of shrinkage and warpage. Without this data, Moldflow predictions of clamp force and gate freeze-off may deviate from production results by more than 10%, particularly for thin-wall parts with flow-length-to-wall-thickness ratios above 150:1.