| HS Code | 377854 |
| Density | 0.918 g/cm³ |
| Meltindex | 1.0 g/10 min (190°C/2.16 kg) |
| Comonomer | Butene-1 |
| Meltingpoint | 122 °C |
| Vicatsofteningpoint | 93 °C |
| Tensilestrengthatyield | 10.3 MPa |
| Tensilestrengthatbreak | 25.5 MPa |
| Elongationatbreak | 800% |
| Flexuralmodulus | 241 MPa |
| Dartdropimpact | 120 g |
| Elmendorftearstrengthmd | 300 g |
| Elmendorftearstrengthtd | 500 g |
| Haze | 10% |
| Gloss | 80% |
As an accredited LyondellBasell CP810-01 Natural Linear, Low-Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell CP810-01 Natural LLDPE resin is supplied in 25 kg polyethylene bags, palletized and stretch-wrapped, or 1,000 kg bulk bags. |
| Container Loading (20′ FCL) | 20′ FCL container loading: LyondellBasell CP810-01 Natural Linear Low-Density Polyethylene, 25 kg bags, palletized, stretch-wrapped, securely stowed for ocean transport. |
| Shipping | LyondellBasell CP810-01 Natural LLDPE ships as non-hazardous resin pellets. Standard packaging is 25 kg polyethylene bags, palletized and stretch-wrapped, often 1,000–1,250 kg per pallet. Bulk shipments use trucks or rail hopper cars. Store dry, away from sunlight and ignition sources; follow the SDS. |
| Storage | Store LyondellBasell CP810-01 Natural LLDPE indoors in a cool, dry, well-ventilated area, away from direct sunlight, heat, flames, and strong oxidizers. Keep original bags or containers closed, clean, and palletized to prevent moisture, dust, and contamination. Avoid prolonged temperatures above 50°C and UV exposure. Use first-in/first-out rotation, good housekeeping, and grounded handling equipment to control static. |
| Shelf Life | Shelf life is typically 24 months from manufacture when stored unopened in cool, dry, well-ventilated conditions, away from sunlight. |
On cast pallet-stretch film lines producing 20–23 µm machine gauge, CP810-01 Natural is fed neat or at 70–85 wt% in the core layer of a three-layer A/B/C structure. Barrel temperatures are profiled from 40 °C in the feed zone to 245–260 °C at the adapter and die. Melt temperature before the final screen pack is held between 255 °C and 270 °C. A 0.7–0.9 mm die gap on a 275–320 °C die body is paired with a 15–20 °C chrome chill-roll surface. Line speed is set at 250–450 m/min. The natural resin has no slip additive; surface cling is supplied by an outer layer containing polyisobutylene or plastomer tackifier. The molecular weight distribution of CP810-01 Natural is broad enough to reduce polymer buildup on the air knife but not so broad as to eliminate edge neck-in. At line speeds above 400 m/min edge trim can increase from 8 % to 12 % because shear stress at the die lip reduces web width. The core layer elongation at break is evaluated per ASTM D882-18; converters often set 500 % as a lower control limit for 20 µm film. Elmendorf tear above 450 gf in the transverse direction is used as a release criterion for machine-wrap grades. Pre-drying is unnecessary below 60 % relative humidity. When outdoor storage has produced surface condensation, a 2 h hot-air pass at 60 °C prevents feed-throat gassing. The terminal pallet wrap is slit to 450 mm or 500 mm rolls and used in automated pre-stretch machines. Pallet retention performance is validated per ASTM D5459-18. The critical production bottleneck is die-lip plate-out; oxidized gel particles can accumulate after 8–12 h and leave visible web stripes if the lip is not purged.
| Property | Test method | Typical control band | Processing implication |
|---|---|---|---|
| Melt volume-flow rate | ISO 1133-1:2022 | 0.95–1.10 g/10 min | Higher melt flow reduces cast film neck-in; lower melt flow supports blown film bubble stability. |
| Density | ISO 1183-1:2019 | 0.916–0.920 g/cm³ | Density below 0.920 g/cm³ supports low-temperature toughness and seal initiation. |
| Elmendorf tear MD/TD | ASTM D1922 | 120–220 gf for 50 µm blown film | TD tear is increased by raising blow-up ratio above 2.2:1. |
| Dart drop impact | ASTM D1709-16a, Method A | 90–160 g for 25 µm blown film | Impact loss below 90 g indicates over-orientation at low frost-line height. |
| Puncture resistance | ASTM D5748-19 | 25–40 J/mm for 70–100 µm cast stretch hood film | Values below 25 J/mm at 23 °C signal insufficient core-layer gauge or excessive LDPE dilution. |
Heavy-duty sacks for mineral fillers, polymer pellets, and construction chemicals are blown on high-stalk lines at 70–120 kg/h. CP810-01 Natural is dry-blended with 10–25 wt% high-pressure LDPE to improve melt strength and bubble stability. Die gap is set at 1.4–2.0 mm. Blow-up ratio is held between 2.0:1 and 2.8:1. Film gauge is 100–180 µm. Bubble cooling air is supplied at 8–14 °C with a frost-line height of 6–10 die diameters. The preferred extruder is a 30:1 L/D barrier screw with a compression ratio of 2.5–3.0; a general-purpose screw frequently produces surge that appears as bubble weave. Cold-temperature puncture retention is governed by the beta-relaxation behavior of the amorphous phase. In ethylene-butene LLDPE of this density class, puncture energy tested under ASTM D5748-19 declines more sharply below −20 °C than in an ethylene-octene plastomer-rich layer. Fillers and mineral packagers moving frozen aggregates must validate terminal sacks in a cold chamber at the intended handling temperature. Heat-seal jaw temperature is set at 140–150 °C; seal strength above 900 N/50 mm is measured per ASTM F88/F88M-21. The natural grade contains no UV protection; carbon-black concentrate is added at 15–30 wt% when the sack is used as an outdoor FIBC liner or tarpaulin. The terminal product is used in valve sacks, open-mouth sacks, and sewn-closure liners for bulk shipment.
In extrusion lamination of oriented polypropylene or polyester to aluminum foil, CP810-01 Natural is extruded as a 15–25 µm sealant web. Melt temperature is kept at 280–300 °C to promote oxidative adhesion to the primed substrate. Residence time in the die, adapter, and transfer pipe should not exceed 10 min; above this threshold gel formation from long-chain branching and oxidation becomes visible as coat-weight defects. The air gap is maintained at 80–130 mm. Nip pressure at the cooling roll is 60–80 N/mm. Bond strength is measured per ASTM F904-16 after 24 h cure; adhesion fails when corona treatment at the point of contact is below 40 dyn/cm. The grade is used as the sealant web in dry-food laminates and retort pouch structures only after the converter verifies the food-contact status under FDA 21 CFR 177.1520 and regional migration requirements. Coefficient of friction is managed by downstream application of oleamide or silica from a flexo station because the natural resin is not pre-compounded with slip or antiblock. Die-lip edge tear is controlled by using a 40 mm purge collar and a die-bolt profile held to ±0.02 mm. The terminal flexible packaging structure requires the converter to monitor seal initiation temperature; the LLDPE sealant web typically initiates sealing at 95–105 °C, which allows lamination with heat-sensitive inks.
Agricultural towers converting CP810-01 Natural into 180–250 µm silage covers require 3–6 wt% HALS-based UV stabilizer masterbatch and 2–4 wt% black or white pigment concentrate. The base resin is selected without a built-in UV package so the same feedstock can be recompounded for different regional exposure zones. The die diameter is 300–500 mm. Blow-up ratio is 2.2:1–3.0:1. Frost-line height is raised to 10–15 die diameters to increase machine-direction toughness. Tear propagation is tested under ASTM D1922 after 1,000 h QUV weathering per ASTM G154-16. The product specification requires retention of at least 50 % of original elongation at break after 6 months of outdoor exposure. Dispersion of the HALS masterbatch is the critical mixing parameter; on extruders with L/D below 28:1 additive domains remain undispersed and form surface pits that permit silage acid permeation. Surface water on pre-stored resin can cause pinholes; a vented feed pocket and hot-air drying at 55–65 °C for 1–2 h are used when storage is above 50 °C or 80 % relative humidity. Long-life greenhouse film requires a separate thermal stabilizer evaluation because natural grades are generally supplied with only processing stabilization. The terminal products are bunker silage covers, clamp covers, and nursery side-sheet films.
High-speed stretch hood lines running 300–450 m/min require a 90–120 mm extruder with 33:1 L/D. Die temperature is raised to 265–280 °C to reduce melt fracture at the lip. The extruded web is drawn downward onto a 12–16 °C chill-roll stack. Air knife pressure is regulated at 0.2–0.5 bar to prevent web lift above 350 m/min. The grade is used in the core layer at 75–85 wt% with an outer layer of metallocene LLDPE or octene-based plastomer for puncture. The broader molecular weight distribution of CP810-01 Natural produces greater neck-in than a metallocene-only structure; edge trim can increase from 8 % to 12 % when the die gap exceeds 1.0 mm. The terminal stretch hood film is specified at 70–100 µm gauge and is used for pallet covers in building materials and appliance logistics. Puncture energy measured per ASTM D5748-19 is typically in the 25–40 J/mm range at 23 °C; at −10 °C the same structure may fall to 20–24 J/mm. Converters shipping into cold storage must perform a cold-chamber drop test per ISTA 3A; the low-temperature result depends more on the plastomer content in the outer layer than on the core resin. Film blocking is controlled by winding tension below 0.5 N/mm because the natural core has no antiblocking agent.
Compounding of 40–60 % carbon-black masterbatches using CP810-01 Natural as carrier resin is performed on twin-screw extruders with 40:1 L/D and 12–14 kW/kg specific energy input. The low melting point of the LLDPE carrier allows the concentrate to be diluted into blown film lines without generating excessive shear heating. The carrier is selected because its density of 0.916–0.920 g/cm³ is close to the dilution hosts; this limits layer-to-layer density mismatch in thick films. Carbon black is introduced through a side feeder at barrel section 6 after the polymer is completely melted. The terminal concentrate is pelletized through an underwater die at 180–200 °C and dried to below 0.08 % moisture. The masterbatch is used in black agricultural films, conductive packaging, and geomembrane liners. A converter-level failure mode appears when the concentrate is let down below 4 %; carbon-black dispersion measured per ASTM D5596-03 weakens and surface roughness increases. The natural carrier has no slip package, so concentrated film can increase die-lip blocking if the let-down ratio exceeds 12 % in high-speed cast film.
Competitive LyondellBasell CP810-01 Natural Linear, Low-Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell CP810-01 Natural Linear Low-Density Polyethylene is an unpigmented, uncompounded thermoplastic olefin resin classified under ASTM D883 as a linear low-density polyethylene. The term “Natural” identifies the absence of deliberately added colorant or carbon black; it does not imply that the resin is free of the primary antioxidant package normally used for melt stabilization. The polymer backbone is essentially linear, with short-chain branches inserted by an alpha-olefin comonomer, and this architecture separates CP810-01 Natural from high-pressure low-density polyethylene produced in autoclave or tubular reactors with long-chain branching. The product code alone does not define comonomer type, molecular weight distribution, or stabilizer loading, and the converter should treat the current LyondellBasell technical data sheet as the controlling document. Published data for this specific configuration is limited; the numerical ranges discussed below are representative of the natural LLDPE class rather than grade-specific certificate values. The resin is nonpolar and will not melt-blend into polar barrier polymers such as ethylene-vinyl alcohol, polyamide, or polyethylene terephthalate without a tie-layer or compatibilizer. Outdoor use requires additional ultraviolet stabilization unless the data sheet confirms otherwise.
Compared with high-density polyethylene grades having density above 0.940 g/cm³, this linear low-density class shows lower flexural modulus and lower Vicat softening temperature but higher elongation and greater resistance to environmental stress cracking under constant strain. Compared with high-pressure LDPE, the linear backbone provides higher tensile strength and dart impact, but lower melt elasticity and bubble stability in blown film. If CP810-01 Natural is produced with a butene comonomer, switching to a hexene or octene LLDPE may improve tear strength and environmental stress-crack resistance, while the reverse switch may reduce melt pressure and improve drawdown. The comonomer and catalyst chemistry should be verified from the LyondellBasell datasheet before relying on these generalized comparisons.
Replacing a high-pressure LDPE or a butene-copolymer LLDPE with CP810-01 Natural should be handled as a process change, not a drop-in substitution. Melt flow rate at 190 °C/2.16 kg is a single-point viscosity indicator and does not predict pressure under high shear. Capillary rheometry according to ASTM D3835 or oscillatory shear according to ISO 6721-10 provides the shear-viscosity curve needed for screw and die sizing. LLDPE of this class generally has a narrower shear-sensitivity envelope than autoclave LDPE; the practical result is that motor load and melt temperature rise faster as screw speed increases. On a 40 mm single-screw extruder with a 30:1 L/D barrier screw, wall-mounted thermocouples can understate the melt temperature at the screw tip by 8–12 °C during high-speed operation. Adapter head pressure, specific energy consumption in kWh/kg, and screw recovery time should be logged before and after the change. A stepwise trial sequence of 5 wt%, 50 wt%, and 100 wt% CP810-01 Natural reduces the risk of drive-train overload when the incumbent grade is a fractional-melt LDPE with high long-chain branching.
In extrusion tooling with narrow die gaps, LLDPE exhibits a lower critical shear rate for sharkskin melt fracture than high-pressure LDPE at similar melt temperature because the linear chains do not strain-harden strongly in the die entry. The onset of sharkskin can be suppressed by raising die temperature, increasing die gap, or using an external fluoropolymer processing aid at 200–1000 ppm. Processing aids migrate to the die wall and reduce the wall-slip threshold, but their use must be reviewed for food-contact compliance in the finished article. Die-lip deposits and gel formation can be monitored by pressure-fluctuation amplitude; an increase of 5 % or more in peak-to-peak head pressure at constant screw speed suggests melt degradation or additive plate-out.
During injection molding, the linear structure produces lower melt elasticity than high-pressure LDPE, which reduces die swell but can promote jetting if the gate land is too short or if fill velocity is set above the critical shear rate for melt fracture. Barrel profiles of 190–240 °C and mold temperatures of 10–30 °C are common starting points for general-purpose tooling. A general-purpose polyolefin screw with a compression ratio of 2.5:1–3.5:1 is usually acceptable, but high-shear barrier screws can generate excessive melt temperature if back pressure exceeds 10 bar. Back pressure of 5–10 bar and screw surface speed of 0.3–0.6 m/s are reasonable LLDPE starting points, with the exact setting adjusted to maintain a stable cushion of 2–5 mm. Holding pressure should be established by gate-seal time study rather than fixed time, because premature hold-pressure release causes sink marks in thick sections and voiding at rib intersections.
Blown film operations expose the lower extensional strain hardening of natural LLDPE, and bubble stability at equal die gap and blow-up ratio is generally lower than for high-pressure LDPE. Die gaps of 1.5–2.5 mm and blow-up ratios of 2.2–3.0 are common adjustments, with 10–20 wt% high-pressure LDPE added when bubble flutter persists. Each increment of LDPE lowers tensile strength and puncture resistance, so the blend ratio should be fixed by falling-dart impact testing under ASTM D1709 Method A or B rather than by visual clarity alone. Excessive air-ring velocity can destabilize the frost line and create gauge bands, while inadequate internal bubble cooling raises film blocking in natural grades supplied without added antiblock. Surface condensation on cold pellets should be managed by predrying for 2–4 h at 80 °C in a desiccant dryer, although polyethylene itself is not hygroscopic. Melt temperatures above 260 °C increase oxidative degradation; sustained temperatures above 290 °C can generate aldehydes and shift organoleptic performance in food-sensitive applications.
The property envelope of natural LLDPE is governed by density, comonomer distribution, molecular weight, and molecular weight distribution. Table 1 lists representative ranges for the class, not specification limits for CP810-01 Natural. A certificate of analysis may show lot-to-lot variation within the manufacturer’s specification but outside the ranges below.
| Property | Test Method | Typical Range |
| Nominal density | ASTM D792 / ISO 1183-1 | 0.915–0.925 g/cm³ |
| Melt mass-flow rate | ASTM D1238 / ISO 1133-1, 190 °C/2.16 kg | 0.8–2.0 g/10 min |
| Tensile yield strength | ASTM D638 Type IV, 50 mm/min | 8–14 MPa |
| Tensile break strength | ASTM D638 Type IV, 50 mm/min | 20–38 MPa |
| Elongation at break | ASTM D638 Type IV | 600–900 % |
| Flexural modulus, 1 % secant | ASTM D790 / ISO 178 | 220–360 MPa |
| Vicat softening temperature, A50 | ASTM D1525 / ISO 306 | 90–105 °C |
| Melting peak temperature | ASTM D3418 / ISO 11357-3 | 120–126 °C |
For critical articles, incoming inspection should include density by ASTM D792, melt flow rate by ASTM D1238, and notched Izod impact by ASTM D256. The test method and conditioning history should be fixed in the purchasing specification to avoid interlaboratory bias. Mechanical values obtained on injection-molded plaques conditioned at 23 °C and 50 % relative humidity under ASTM D618 should not be extrapolated to blown or cast film, because orientation, cooling rate, and tie-molecule concentration differ. Secant modulus measured at 1 % strain by ASTM D790 is not a substitute for creep testing when the part is under continuous load; ISO 899-1 provides tensile creep data.
Gamma sterilization at 25–40 kGy can induce free-radical oxidation and yellowing in natural LLDPE if the grade does not contain a radiation-resistant additive package. Ethylene oxide and electron-beam sterilization are possible alternatives, but compatibility of the packaging and sealing layers must be validated under ISO 11135 or ISO 11137 as applicable. A natural unpigmented appearance does not by itself confer medical or food-contact compliance.
In multi-cavity cold-runner tools, weld lines form where melt fronts meet at low temperature and limited pressure. General-purpose LLDPE can exhibit weld-line tensile strength reductions of 20–40 % relative to parent material, a loss that becomes unacceptable in living hinges, snap-fit features, or pressure-containing closures. Mold-filling simulation should be calibrated with Cross-WLF viscosity coefficients from the supplier’s rheology data, and pressure-specific-volume-temperature data can be measured by piston-cylinder dilatometry according to ISO 17744. If simulation predicts a weld line in a structural region, the gate should be moved or a flow leader added before tool steel is cut. When gate movement is not possible, increasing melt temperature by 10–15 °C and reducing injection velocity can broaden the flow front and improve intermolecular diffusion, but the result must be validated by part-level burst testing or drop-weight impact testing, not by standardized tensile specimens alone.
Shallow sections below 1 mm are particularly sensitive to flow hesitation, and sequential valve gating should be considered when cavity-to-cavity filling imbalance exceeds 5 % by mass or when shot-to-shot variation in cushion exceeds 2 mm. Injection-molding machines with closed-loop transfer from velocity to pressure control require repeatable switch-over position, measured by screw displacement, to avoid short shots and flash in the same cavity set. Regrind levels above 20 wt% can shift melt flow rate and lower impact strength; regrind use should be validated with a melt flow rate check at 190 °C/2.16 kg and a notched Izod test according to ASTM D256.
Compliance claims for CP810-01 Natural in food-contact and regulated applications require the converter to verify that the finished article meets the applicable jurisdiction. Olefin base resins may be covered by FDA 21 CFR 177.1520 for specified food types and conditions, but the manufacturer’s food-contact statement must identify the grade and any limitations on fatty food or hot-fill. In the European Union, plastics intended for food contact are assessed under Regulation (EU) No 10/2011, with overall migration measured by EN 1186-1 and specific migration of comonomer and additives measured by EN 13130 methods. For electrical and electronic equipment, the finished part is subject to RoHS Directive 2011/65/EU, although unfilled natural polyethylene is not a significant source of lead, cadmium, mercury, or brominated flame retardants. A supplier declaration under REACH Annex XVII should be obtained if the grade is colored downstream, because pigment concentrates may introduce restricted substances.
| Requirement | Reference | Converter Verification |
| Olefin polymer base resin | FDA 21 CFR 177.1520 | Supplier food-contact statement; finished-article migration testing for fat or hot-fill |
| EU food-contact plastics | Regulation (EU) No 10/2011 | Overall migration by EN 1186-1; specific migration by EN 13130 |
| Restricted substances in electrical/electronic equipment | RoHS Directive 2011/65/EU | Supplier declaration; X-ray fluorescence screening after colorant addition |
| Resin specification and contamination | ASTM D4976 | Density, melt flow rate, and visual contamination certificate |