| HS Code | 244773 |
| Density | 1.19 g/cm³ |
| Hardness | 63 Shore D |
| Tensile Strength At Break | 32 MPa |
| Elongation At Break | 500% |
| Flexural Modulus | 220 MPa |
| Tear Strength | 130 kN/m |
| Melting Point | 200 °C |
| Vicat Softening Temperature | 170 °C |
| Brittleness Temperature | -70 °C |
| Melt Flow Rate | 10 g/10 min (230 °C/2.16 kg) |
| Water Absorption | 0.5% |
| Mold Shrinkage | 1.5-2.0% |
As an accredited LG Chemical Keyflex® PBT Unfilled BT-1063D factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LG Chemical Keyflex® PBT Unfilled BT-1063D is supplied in 25 kg moisture-resistant bags, palletized for industrial handling and storage. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): 20′ FCL loaded with 25 kg bags of LG Chemical Keyflex® PBT Unfilled BT-1063D, palletized and secured. |
| Shipping | LG Chemical Keyflex® PBT Unfilled BT-1063D is shipped as dry, solid thermoplastic pellets in sealed moisture-barrier bags or containers. Handle as non-hazardous industrial polymer, protect from moisture, heat, contamination, and packaging damage. Store cool and dry; refer to SDS and applicable transport regulations. No special dangerous-goods classification normally applies. |
| Storage | Store LG Chemical Keyflex® PBT Unfilled BT-1063D in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and strong oxidizers. Keep containers tightly closed to prevent moisture ingress and contamination. Protect from dust and physical damage, and practice good housekeeping. Use appropriate PPE when handling. |
| Shelf Life | Shelf life is typically 24 months from manufacture when stored unopened in a dry, cool, well-ventilated area away from direct sunlight. |
Competitive LG Chemical Keyflex® PBT Unfilled BT-1063D prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LG Chemical Keyflex® PBT Unfilled BT-1063D is an unreinforced polybutylene terephthalate injection-moulding resin supplied by LG Chemical. Under ISO 1043-1:2011, the base polymer is designated PBT. The unfilled classification indicates that the formulation contains no glass fibre, mineral filler, or flame-retardant filler at meaningful loading. This absence of reinforcement influences nearly every downstream property relevant to moulding, part design, and end use. The following text addresses the grade in terms of datasheet properties, processing limits, comparative performance against filled PBT and alternative thermoplastics, and regulatory boundary conditions. All numeric values are representative published data or common industry practice unless a specific certificate of analysis is cited. Lot-specific values should be verified against the manufacturer’s documentation before tooling release or production qualification.
Table 1 consolidates representative values from publicly available product data for BT-1063D. The values are not specification limits; they are typical values that must be confirmed against the received batch certificate of analysis. Where a test method is not referenced, the value is an approximate commercial range for unfilled PBT injection-moulding grades of medium flow.
| Property | Value | Test method |
|---|---|---|
| Density | 1.31 g/cm³ | ISO 1183-1:2019 |
| Melt mass-flow rate | 30 g/10 min at 250 °C / 2.16 kg | ISO 1133-1:2022 |
| Mould shrinkage, flow direction | 1.5–2.0 % | ASTM D955-08 |
| Water absorption, 23 °C / 24 h | 0.07–0.08 % | ISO 62 |
| Tensile strength | 55 MPa | ISO 527-1/2 |
| Tensile elongation at break | >50 % | ISO 527-1/2 |
| Flexural modulus | 2400 MPa | ISO 178 |
| Flexural strength | 80 MPa | ISO 178 |
| Charpy notched impact strength, 23 °C | 3.0 kJ/m² | ISO 179-1/1eA |
| Heat deflection temperature, 1.8 MPa | 60 °C | ISO 75-1/2 |
| Flammability class, 0.8 mm | HB | UL 94 |
The medium-flow rheology of BT-1063D is reflected in a melt mass-flow rate of approximately 30 g/10 min. This flow class permits short filling times in multi-cavity connector and sensor housings, but it is not equivalent to high-flow PBT grades used for micro-moulding or extremely thin wall sections below 0.4 mm. The crystallinity-dependent mechanical values — flexural modulus near 2400 MPa and tensile strength near 55 MPa — are consistent with unfilled PBT rather than glass-filled polyester compounds. Because elongation at break exceeds 50 %, the resin retains ductility at room temperature; however, the transition to brittle behaviour is dependent on notch radius, moulding condition, and service temperature. The polymer solidifies from the melt as a semicrystalline matrix, and the degree of crystallinity is directly influenced by mould temperature and cooling rate.
Processing of BT-1063D is governed by hydrolytic degradation rather than purely thermal degradation. PBT is a polyester; above the melt point, residual water attacks ester linkages in the polymer backbone. With a target residual moisture content not exceeding 0.02 % at the feed throat, hydrolytic chain scission is minimised, but barrel residence time at melt temperatures of 250–260 °C must still be controlled. On production-scale machines, the practical upper boundary is commonly 10 min total residence time when the barrel is at full temperature. Excessive residence produces a measurable loss in melt viscosity, darkening of the purge, and acetaldehyde-like degradation odours. The effect is accelerated in hot-runner systems; manifold and nozzle temperatures should not exceed 260 °C unless the tool is equipped with narrow-diameter channels and short gate-to-cavity distances.
Closed-loop hopper dryers with desiccant beds are required. Drying at 120 °C for 3–5 h to a dew point of −30 to −45 °C reduces moisture below 0.02 %. Conveying from the dryer to the feed throat should use dry air or nitrogen if ambient relative humidity exceeds 60 %. Vacuum ovens without sufficient airflow do not reliably achieve the target moisture level in high-humidity warehouses. Regrind levels above 20 % are generally not recommended for unfilled PBT unless the regrind has been dried to the same moisture specification. Production-floor experience indicates that splay on the part surface, weak weld lines, and intermittent terminal-retention failures are often the first visible indicators of moisture damage. A moulded part may appear dimensionally acceptable after start-up but fail mechanical testing because hydrolysis has reduced molecular weight. Monitoring melt mass-flow rate before and after drying provides a practical check; an increase of more than 10–15 % relative to the virgin baseline after prolonged drying may indicate molecular-weight loss rather than improved flow.
Melt-temperature profiles for BT-1063D on a general-purpose 20:1 L/D screw are typically set with the rear zone at 230–240 °C, the centre zone at 240–250 °C, the front zone at 250–260 °C, and the nozzle at 250–260 °C. A shallow metering depth and compression ratio of 2.0:1 to 2.5:1 are adequate. Back pressure is maintained at 0.3–0.7 MPa; higher back pressure can increase shear heating and shorten effective residence time but may cause screw recovery delays in large mouldings. Injection speed is selected for rapid cavity filling without jetting. For thin-wall connectors, linear injection velocities of 50–100 mm/s are common, while slower speeds are used for thick-section housings to avoid voids and sink marks. Hold pressure is typically 50–70 % of injection peak pressure. Gate freeze must be verified by part weight stabilisation, because PBT crystallises rapidly and the gate seals quickly at mould temperatures below 80 °C.
Mould temperature is maintained at 40–80 °C. At the lower end, cooling is rapid and cycle time decreases, but underdeveloped crystallinity can produce dimensional drift during later thermal ageing. At the upper end, crystallinity approaches its maximum and the part shows better resistance to post-moulding shrinkage. Tool temperature differentials across the cavity should be kept within ±5 °C because uneven crystallisation in unfilled PBT creates differential shrinkage and unsupported warpage in flat connector bodies. Unfilled PBT mould shrinkage of 1.5–2.0 % is higher and more isotropic than glass-filled PBT. For flat connectors, shrinkage in the flow direction is usually lower than transverse direction; unfilled grades can show differential shrinkage of 0.1–0.3 % between flow and cross-flow. Dimensional inspection should be delayed for 24–48 h after ejection because post-mould shrinkage can continue as crystallinity slowly develops.
In electrical and electronic components, unfilled PBT retains advantages in flow, elongation, and moisture resistance. The 0.07–0.08 % water absorption after 24 h at 23 °C per ISO 62 is substantially lower than that of unreinforced PA66, which commonly absorbs about 2.5 % under similar conditions. As a result, connectors moulded from BT-1063D exhibit less humidity-induced expansion and less variation in electrical creepage distances than polyamide alternatives. This behaviour is relevant in automotive wiring-harness connectors where terminal retention force and pitch stability are required across seasonal humidity cycles.
Tensile elongation above 50 % permits snap-fit arms and latches to deflect during assembly. However, unfilled PBT is notch-sensitive. Gate and ejector marks on loaded surfaces can initiate cracks if moulded-in stress exceeds the local yield. For latch bases, a minimum radius of 0.5 mm and generous draft are used. Weld-line strength is lower than un-welded tensile strength; when weld lines are unavoidable in pin arrays, sequential valve gating or flow leaders can reposition the knit line away from the load path. On production-scale tools, cavity-to-cavity fill imbalance in hot-runner systems has been observed to produce intermittent terminal retention failures; this is addressed by balancing runner lengths and using in-cavity pressure sensors to control switchover.
UL 94 classification for this grade is HB; for live parts requiring V-2 or V-0, a flame-retardant PBT grade is required. Published data for this specific configuration is limited for long-term high-voltage tracking, so comparative tracking index values should be obtained from the supplier rather than assumed from general unfilled PBT literature. Multi-cavity tools with four or more cavities require gate placement that prevents convergence of melt fronts in the pin-retention area. Weld lines in unfilled PBT are less visible than in glass-filled compounds, but the loss of strength at the weld line can be significant. Sequential valve gating or overflow tabs are used where weld-line integrity is critical.
| Property | Unfilled BT-1063D | GF30 PBT | Test method |
|---|---|---|---|
| Density | 1.31 g/cm³ | 1.53 g/cm³ | ISO 1183-1:2019 |
| Tensile strength | 55 MPa | 130 MPa | ISO 527-1/2 |
| Tensile elongation at break | >50 % | 2–3 % | ISO 527-1/2 |
| Flexural modulus | 2400 MPa | 8500 MPa | ISO 178 |
| Charpy notched impact strength, 23 °C | 3.0 kJ/m² | 9.0 kJ/m² | ISO 179-1/1eA |
| Heat deflection temperature, 1.8 MPa | 60 °C | 205 °C | ISO 75-1/2 |
| Mould shrinkage, flow direction | 1.5–2.0 % | 0.3–0.6 % | ASTM D955-08 |
| Flammability class | HB | HB | UL 94 |
The central difference is stiffness. GF30 PBT increases flexural modulus to approximately 8500 MPa, more than three times the 2400 MPa of unfilled BT-1063D. This stiffness is accompanied by a heat deflection temperature increase from 60 °C to about 205 °C at 1.8 MPa. The trade-off appears in tensile elongation: GF30 PBT fails at 2–3 %, whereas BT-1063D can exceed 50 %. In applications requiring snap-fit assembly or repeated deflection, the unfilled grade is therefore less likely to crack during installation. In contrast, structural brackets or motor supports requiring load at 150 °C are outside the recommended service envelope of unfilled BT-1063D.
Compared to PET, PBT crystallises more rapidly. In moulds at 40 °C, unfilled PET may require nucleating additives or higher mould temperatures to achieve useful crystallinity, while BT-1063D solidifies rapidly and ejects cleanly. PET generally has slightly higher tensile strength and stiffness, but slower crystallisation rates make it less forgiving in complex multi-cavity tools. PBT also has lower melt viscosity at equivalent processing temperatures, permitting lower injection pressure in thin-wall sections. Glass-fibre PBT is preferred when components require load-bearing capability at 150 °C or above. Unfilled BT-1063D at 1.8 MPa HDT/A of approximately 60 °C is not suitable for structural under-hood components near engine exhaust or turbocharger heat sources.
Regulatory confirmation for BT-1063D must be obtained from the supplier’s documentation for each grade and region. The base PBT chemistry is generally included in generic clearances when produced with authorised monomers; however, the specific product’s stabilisers, processing aids, and colour packages determine final compliance. Under European Union REACH, the manufacturer is responsible for pre-registration and Safety Data Sheet disclosure. Under RoHS Directive 2011/65/EU, PBT resins are evaluated for lead, cadmium, mercury, hexavalent chromium, PBB, and PBDE content at the homogeneous-material level. For electrical parts, UL yellow card data for the specific grade and thickness should be used. The unfilled grade is typically classified HB under UL 94 at 0.8 mm. When a V-0 or V-2 flame-retardant classification is required, a flame-retardant PBT grade must be substituted because BT-1063D does not contain halogenated or phosphorus-based flame retardants.
Material handling and storage limitations are operationally relevant. Avoid combination with amine-based additives or colour concentrates containing unknown carriers; amines may catalyse ester interchange or cause discoloration. Avoid long-term storage in unsealed containers at relative humidity above 60 %. Food-contact evaluation under FDA 21 CFR 177.1660 may be possible for unfilled PBT, but only if the grade is listed by the manufacturer and the end-use conditions are covered. Do not assume that BT-1063D is food-contact approved without written certification.
Batch-to-batch control in injection moulding usually includes melt mass-flow rate by ISO 1133-1:2022, density by ISO 1183-1:2019, and moisture analysis. A shift in MFR beyond 10 % should trigger retention and drying review. Avoid contamination with polyamide or PC/ABS; even small amounts of PA can cause layer delamination and inconsistent shrinkage. Published data for outdoor UV ageing of this specific unfilled grade is limited. Parts exposed to direct sunlight require black formulations with UV stabiliser packages or opaque coatings. Do not use this product as a direct substitute for flame-retardant PBT in regulatory electrical applications without completing end-product flammability and glow-wire testing to the applicable IEC 60695 series.