Lg Chemical Keyflex Pbt Unfilled Bt 1030d

LG Chemical Keyflex® PBT Unfilled BT-1030D

    • Product Name: LG Chemical Keyflex® PBT Unfilled BT-1030D
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 564400
    Density 1.31 g/cm³
    Water Absorption 0.08%
    Mold Shrinkage 0.7-1.0%
    Tensile Strength At Break 50 MPa
    Elongation At Break 30%
    Flexural Modulus 2300 MPa
    Flexural Strength 80 MPa
    Notched Izod Impact Strength 4 kJ/m²
    Hdt At 0 45 Mpa 150 °C
    Hdt At 1 8 Mpa 60 °C
    Melting Point 225 °C
    Volume Resistivity 1E16 ohm·cm
    Dielectric Strength 20 kV/mm

    As an accredited LG Chemical Keyflex® PBT Unfilled BT-1030D factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing LG Chemical Keyflex® PBT Unfilled BT-1030D is supplied in 25 kg moisture-barrier bags, palletized for secure industrial storage and handling.
    Container Loading (20′ FCL) 20′ FCL container loaded with LG Chemical Keyflex® PBT Unfilled BT-1030D in standard export packaging, palletized, secured, and evenly distributed.
    Shipping Shipped as pelletized resin in sealed moisture-barrier 25 kg bags, palletized and stretch-wrapped. Store in a cool, dry, ventilated area away from sunlight, heat, and moisture. Handle per SDS; generally non-hazardous for transport. Avoid bag damage and contamination.
    Storage Store LG Chemical Keyflex® PBT Unfilled BT-1030D in its original sealed containers or bags in a cool, dry, well-ventilated warehouse, protected from direct sunlight, heat, and moisture. Keep away from ignition sources and strong oxidizers. Reseal opened packages promptly, rotate stock, and follow supplier drying recommendations before processing.
    Shelf Life Typical shelf life is 12 months in original sealed packaging, stored dry, below 30°C, away from moisture and direct sunlight.
    Free Quote

    Competitive LG Chemical Keyflex® PBT Unfilled BT-1030D prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    LG Chemical Keyflex® BT-1030D is an unfilled polybutylene terephthalate (PBT) injection-molding resin positioned in the medium-flow region of the Keyflex® PBT portfolio. The grade is supplied as pellets formulated without glass fiber or mineral filler, so the melt-rheological response is governed primarily by the polyester backbone and its molecular weight distribution. Manufacturer technical data report a melt volume-flow rate at 250 °C under a 2.16 kg load of 18 cm³/10 min when measured according to ISO 1133-1:2022. Density under ISO 1183-1:2019 is approximately 1.31 g/cm³. These two values define the design space: the resin is fluid enough for multi-cavity electrical parts but remains below the high-flow grades used for sub-0.5 mm wall connectors or high-cavitation micro-molding.

    What separates an unfilled medium-flow PBT from reinforced, impact-modified, and flame-retarded grades?

    At the property level, an unfilled PBT of this class exhibits flexural modulus below 2500 MPa under ISO 178:2019, while a 30 wt% glass-fiber-reinforced PBT commonly exceeds 8000 MPa. BT-1030D is therefore selected for parts that do not require structural stiffness but must fill complex geometries with lower melt pressure and reduced fiber-induced anisotropy. Its tensile strength at yield is approximately 54 MPa under ISO 527-2:2012, and failure is ductile with elongation at break above 100 % in some reported datasets; published data for this specific configuration should be confirmed against the current manufacturer certificate. The absence of glass fiber also removes a principal cause of warpage in reinforced grades: differential shrinkage along flow and transverse directions. Whereas a 30 wt% glass-fiber PBT may show flow-direction shrinkage near 0.3 % and transverse shrinkage near 1.0 %, the unfilled grade typically shows mold shrinkage in the range 1.7 %–2.0 % under ISO 294-4:2018.

    Compared with impact-modified unfilled PBT, BT-1030D displays a notched Charpy impact value around 4 kJ/m² at 23 °C under ISO 179-1:2010. Snap-fit designs requiring ductile fracture at low temperatures or high strain-rate loading may require an impact-modified grade. Against flame-retarded grades, an unfilled, unmodified PBT generally carries only a UL 94 HB rating; V-0 classification at thin wall sections requires halogenated or phosphorus-based flame-retardant packages that alter flow, mold deposit behavior, and thermal stability.

    Within unfilled PBT ranges, melt volume-flow rate values typically span 12 cm³/10 min to 30 cm³/10 min under the same ISO condition. BT-1030D at 18 cm³/10 min therefore sits near the middle of that distribution. This positioning reduces short-shot risk in thin-wall fill relative to low-flow extrusion grades, but it does not match the filling behavior of a 30 cm³/10 min high-flow PBT in sub-0.5 mm micro-connector geometries. High-flow grades usually sacrifice impact and long-term hydrolysis resistance because lower molecular weight translates into fewer chain entanglements; the medium-flow selection retains a measurable margin of ductility for small snap-fit arms.

    Processing behavior is dominated by two factors: rapid crystallization at quench-rate-dependent temperatures and moisture-induced ester hydrolysis. In production, a desiccant dryer capable of delivering air at a dew point below -30 °C is required when pellets are exposed to ambient humidity above 50 % RH. Drying at 120 °C for 3 h to 4 h reduces pellet moisture to a target below 0.02 %. Moisture above 0.03 % at the hopper produces splay, nozzle drool, and a progressive loss in tensile strength because hydrolytic chain scission reduces molecular weight. On reciprocating-screw machines with L/D 20:1 and compression ratio 2.2:1, barrel settings range from 235 °C at the rear zone to 250 °C at the front and nozzle. Melt temperature should be maintained between 245 °C and 260 °C. Extended residence above 260 °C causes discoloration and a reduction in elongation at break; accumulated melt residence time should not exceed 8 min for this grade.

    Mold temperature is the primary control for crystallinity development. A mold temperature of 60 °C to 80 °C is recommended for parts requiring stable dimensions and improved heat deflection; lower mold temperatures between 30 °C and 40 °C may be used for fast cycle times but can produce underdeveloped crystallinity, higher post-mold shrinkage, and lower HDT. Injection pressure is typically set between 60 MPa and 100 MPa at the screw tip, with hold pressure adjusted until the cavity pressure transducer records a transfer point at 95 %–98 % of fill volume. Back pressure between 5 MPa and 10 MPa and screw surface speed between 60 min⁻¹ and 120 min⁻¹ maintain melt homogeneity without generating excessive shear heat. Cushion should be kept above 3 mm; shot-weight instability at cushion values below 2 mm has been observed as poor filling repeatability in multi-cavity tools.

    Gate diameter must be at least 50 % of local wall thickness because the gate freezes rapidly once the melt drops below the crystallization temperature, and premature seal prevents packing. For walls between 1.0 mm and 2.5 mm, a round gate diameter of 0.8 mm to 1.2 mm and land length under 1.0 mm are typical. Hot-runner needle valves should be used in place of open sprue bushings when stringing, drool, or gate vestige control is critical.

    Typical injection-molding parameter window for Keyflex® BT-1030D on a general-purpose screw with L/D 20:1
    Parameter Set point Control method or instrument
    Drying temperature 120 °C Desiccant dryer
    Drying time 3–4 h Dew point -30 °C or lower
    Maximum pellet moisture 0.02 % Karl Fischer or moisture analyzer
    Rear barrel 235–245 °C Thermocouple
    Front barrel 250–260 °C Thermocouple
    Melt temperature 245–260 °C Air-shot pyrometer
    Mold temperature 60–80 °C Water temperature control
    Injection pressure 60–100 MPa Screw-tip pressure transducer
    Back pressure 5–10 MPa Hydraulic pressure transducer
    Cushion 3–6 mm Linear position
    Maximum residence time 8 min at 250 °C Shot counter × cycle time

    Property profile, electrical connector suitability, and thermal limits

    In electrical connector housings and relay sockets, BT-1030D is used where median flow, predictable shrinkage, and electrical-insulation performance are adequate for ambient and mildly heated environments. The heat deflection temperature under 1.8 MPa load is approximately 55 °C when tested according to ISO 75-2:2013; continuous load-bearing service above this value is outside the unfilled grade’s mechanical reliability envelope. For parts that must survive reflow soldering above 240 °C, the grade is generally unsuitable unless the process is vapor-phase reflow with controlled dwell below the HDT; high-heat PBT or glass-fiber-reinforced grades are required.

    Typical property data reported for the grade are consolidated in the table below; they should be read as representative values rather than batch-release specification limits.

    Typical property data for Keyflex® BT-1030D, unfilled PBT
    Property Standard Value
    Density ISO 1183-1:2019 1.31 g/cm³
    Melt volume-flow rate ISO 1133-1:2022 18 cm³/10 min
    Tensile strength at yield ISO 527-2:2012 54 MPa
    Tensile elongation at break ISO 527-2:2012 >100 %
    Flexural modulus ISO 178:2019 2300 MPa
    Flexural strength ISO 178:2019 80 MPa
    Notched Charpy impact at 23 °C ISO 179-1:2010 4 kJ/m²
    HDT/A, 1.8 MPa ISO 75-2:2013 55 °C
    Mold shrinkage ISO 294-4:2018 1.7 %–2.0 %
    Water absorption, 24 h ISO 62:2008 0.08 %

    Electrical insurer listing is generally UL 94 HB at 0.8 mm thickness for unfilled and unmodified PBT; comparative tracking index and glow-wire performance must be evaluated on the finished part because additives, colorants, and molding strains affect the result. Published data for this specific grade’s CTI is limited; values for unfilled PBT often exceed 400 V but cannot be assumed without a certification file.

    When the melt is held above 250 °C for more than 8 minutes

    Thermal degradation pathways in PBT shift from reversible ester interchange to irreversible vinyl-ester decomposition as residence time accumulates. In an injection unit, this manifests initially as yellowing and an increase in melt pressure variation; later, tetrahydrofuran-related odours may appear and the melt viscosity decreases through chain scission. Because BT-1030D is unfilled and of medium viscosity, the torque signal may remain inside the machine alarm band while the polymer is already degrading. Shot-to-shot variation in cushion position and nozzle pressure should be interpreted as a residence-time warning, not corrected solely by raising back pressure. The safe response is to reduce barrel temperature to the lower end of the melt window and purge the barrel with a fresh PBT charge. Unlike some glass-fiber-reinforced grades that tolerate brief excursions to 270 °C, the unfilled grade’s degradation threshold is lower because no reinforcing filler moderates shear heating or local overheating. Barrel-temperature profiling should be established with an air-shot pyrometer at start-up, and measured melt temperature should not deviate by more than ±5 °C from the nominal setting when controlled by closed-loop barrel thermocouples. This operational boundary is particularly relevant to hot-runner systems with poorly swept dead zones and to high-cycle molding cells running below 15 % of barrel capacity, where the material spends a large fraction of the cycle in the plastication zone.

    In multi-cavity connector manufacturing, the unfilled grade is commonly selected when nominal wall thickness is 0.8 mm to 2.5 mm and the maximum service temperature under mechanical load remains below 55 °C. The resin fills thin ribs and snap-fit geometries at moderate pressures, but the low notched impact strength of roughly 4 kJ/m² under ISO 179-1:2010 must be designed around by eliminating sharp corners, enlarging radii, and orienting weld lines away from high-strain regions. For terminal blocks, coil bobbins, and switch components, molding trials with water-heated tools at 60 °C reduce part-to-part shrinkage variation by promoting more repeatable crystallinity than low mold-temperature operation. Applications involving continuous exposure to hot water above 60 °C, strong aqueous acids, or organic amines are outside unfilled PBT’s established compatibility envelope because hydrolysis and amine-induced degradation reduce molecular weight. If a part requires V-0 flammability, a specifically flame-retarded Keyflex® grade or a glass-fiber-reinforced PBT with a documented UL Yellow Card classification should be selected instead of BT-1030D.

    Top