| HS Code | 371908 |
| Polymer Base | PBT |
| Glass Fiber Content | 30% |
| Flame Retardant | Yes |
| Hydrolysis Resistance | Yes |
| Density | 1.54 g/cm3 |
| Tensile Modulus | 10500 MPa |
| Tensile Strength | 120 MPa |
| Elongation At Break | 2.0% |
| Charpy Notched Impact Strength 23c | 8 kJ/m2 |
| Hdt A | 200 °C |
| Hdt B | 215 °C |
| Vicat Softening Temperature B | 205 °C |
| Melting Temperature | 225 °C |
| Ul94 Flame Rating | V-0 at 1.5 mm |
| Comparative Tracking Index | 600 V |
| Molding Shrinkage | 0.2-0.6% |
| Water Absorption | 0.4% |
| Melt Temperature Processing | 250-270 °C |
| Mold Temperature Processing | 80-100 °C |
As an accredited Lanxess Pocan® PBT+GF30%-FR-Hydrolytic BF4232HR factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg moisture-proof, foil-lined paper bags, 40 bags per shrink-wrapped pallet (1,000 kg total). |
| Container Loading (20′ FCL) | Lanxess Pocan® PBT+GF30%-FR-Hydrolytic BF4232HR is loaded in a 20-foot FCL container, palletized and shrink-wrapped for safe transport. |
| Shipping | Lanxess Pocan® PBT+GF30%-FR-Hydrolytic BF4232HR is a glass-fiber-reinforced, flame-retardant PBT molding compound supplied as pellets. It is typically non-hazardous for transport (no UN number, DG class, or packing group). Ship in moisture-proof packaging, keep dry, and avoid excessive heat, sunlight, and contamination. |
| Storage | Store Lanxess Pocan® PBT+GF30%-FR-Hydrolytic BF4232HR in its original, sealed packaging in a dry, cool, well-ventilated area, protected from moisture, direct sunlight, heat, and contamination. Keep away from incompatible chemicals and ignition sources. Maintain stable ambient conditions and avoid prolonged exposure to humid air; dry material before processing if prescribed. Observe manufacturer’s shelf-life and handling guidance. |
| Shelf Life | Lanxess Pocan® PBT+GF30%-FR-Hydrolytic BF4232HR has a shelf life of 12 months when stored dry in sealed original packaging below 30°C. |
High-voltage connector systems in battery-electric commercial vehicles place BF4232HR in direct contact with condensed water, glycol-containing coolant leakage and transient heat spikes during fast charging. The specified glass fibre content of 30% by weight provides the creep resistance required to keep contact pitch stable in densely packed busbar carriers, while the flame-retardant package supports a UL 94 V-0 classification when wall sections follow the supplier’s Yellow Card minimum thickness. For production, pellets are pre-dried at 120°C in dehumidified air to a residual moisture below 0.02%. Barrel temperatures are set between 250°C and 270°C, with the nozzle held at 260°C. Tool surface temperature is raised to 90–100°C to accelerate crystallisation and reduce post-moulding shrinkage in long busbar retention features. Injection speed is profiled to avoid jetting at contact retention ribs, and hold pressure is maintained long enough to seal the gate before crystallisation shrinkage creates sink marks at boss areas. A 3500 kN hydraulic clamp unit with a 60 mm screw diameter and 20:1 L/D is representative for multi-cavity connector carriers; the screw should use a low-compression PBT-specific check ring to minimise dead spots. Electrical design verification for moulded parts is run to IEC 60664-1 for creepage and clearance coordination, while comparative tracking index is assessed by IEC 60112. End products include high-voltage interconnects, cell-sense harness connectors and busbar isolation carriers. The failure mode addressed is not bulk ignition but surface tracking after condensation films bridge adjacent terminal positions; hydrolysis-resistant stabilisation is therefore evaluated by damp-heat storage at 85°C/85% RH followed by insulation resistance measurement.
Powertrain sensor housings manufactured from BF4232HR are exposed to continuous thermal soak, vibration from direct engine mounting and intermittent exposure to road spray containing de-icing chloride. The creepage current measured after 85°C/85% RH ageing is governed less by the polymer’s bulk conductivity than by surface deposition of plasticiser breakdown products, chloride salts and mould-release residues. For this reason, the tool process is specified with no external mould-release spray; ejection is controlled by draft angles above 1° and mould surface roughness below 0.4 µm Ra on the sealing ring seat. The 30% glass reinforcement is retained without substitution because sensor housing bosses must withstand thread-forming screw insertion. Pellets are pre-dried at 120°C for 4 h in a desiccant bed dryer with a dew point of −30°C or lower. Barrel profile from hopper to nozzle is 240°C, 255°C, 260°C, 255°C, and mould temperature is held at 100°C to complete crystallisation before ejection. Packing pressure is adjusted to 70–80 MPa at transfer to compensate for high glass fibre content; hold time is set from gate seal time plus 1.5 s. Terminal components include camshaft position sensor housings, boost-pressure sensor flanges and water-in-oil sensor bodies. Compliance verification follows ISO 16750-4 high-temperature durability, USCAR-2 electrical connector performance for terminal fretting, and ISO 527-2 tensile retention after ageing. The operational boundary is chemical contact with strong alkaline underbonnet cleaning agents; PBT-based grades do not tolerate extended immersion at pH above 9. Published data for this specific BF4232HR grade in hot engine oil at 150°C is limited; validation on production tooling is required.
Industrial terminal blocks and relay bases carry continuous current under poorly conditioned panel enclosures in food-processing plants, textile mills and chemical distribution rooms. The primary requirement is creep resistance in thin-section insulating partitions between adjacent poles. The 30% glass fibre level raises heat deflection temperature sufficiently to maintain screw-torque retention during thermal cycling, but it also raises melt viscosity; the injection moulder compensates with 2–3 bar screw back pressure and a 20:1 L/D general-purpose screw with a cored shank. Mould temperature is held at 80–100°C. Regrind is limited to 10% by mass for customer-visible terminal bodies because glass fibre attrition in the sprue/reject reuse stream reduces sharp-edge flash resistance of the partition. Parts are produced via a hot-runner system with individually heated valve gates to prevent stringing across narrow creepage slots. Compliance for terminal blocks is assessed under IEC 60947-7-1, and relay bases are evaluated for glow-wire and tracking to IEC 60695-2-11 and IEC 60112. Terminal products include through-panel terminal strips, relay sockets and current-transformer lead carriers. The limiting operational condition is continuous service above 140°C in poorly ventilated panel corners; at such temperatures oxidation of the flame-retardant package can raise surface leakage current before bulk mechanical properties fail.
| Application segment | Governing test designation | Critical verification quantity | Process boundary |
|---|---|---|---|
| High-voltage busbar carriers | IEC 60664-1, IEC 60112 | Creepage after 85°C/85% RH | Residual moisture below 0.02% |
| Engine-bay sensor housings | ISO 16750-4, USCAR-2 | Tensile retention after hot oil | No external mould-release spray |
| Industrial terminal blocks | IEC 60947-7-1, IEC 60112 | Tracking across pole partitions | Regrind capped at 10% |
| Charging inlet pin retainers | IEC 62196-1, IEC 60068-2-30 | Snap-fit retention after condensation cycling | Two-stage hold pressure |
| Washing machine connectors | IEC 60695-2-12, IEC 60335-1 | Glow-wire margin on latch walls | Melt temperature not above 280°C |
| Photovoltaic junction boxes | IEC 62790, UL 746C | Insulation after damp heat | Hard-surfaced screw required |
| Hot water pump volutes | ISO 527-2, ISO 178 | Flexural retention in hot water | No regrind in pressure boundary |
AC and DC charging inlet housings accumulate condensation when a cold vehicle enters a heated parking garage; subsequent evaporation deposits minerals at the leading edge of contact-pin apertures. BF4232HR is selected for the pin retainer plate and inlet body because the hydrolysis-resistant PBT matrix slows the decline in tensile snap-fit retention after repeated condensation cycles. The 30% glass fibre content keeps the pin retainer plate flat after moisture uptake, but glass orientation at the snap-fit must be controlled by gate placement at a low-shear region. Pellets are pre-dried to 0.02% residual moisture and conveyed with closed resin transfer to avoid moisture entrapment in glass bundles. Melt temperature is held at 250–270°C, mould temperature at 100°C for the fixed half and 80°C for the moving half to balance shrinkage across the deep inlet cavity. Holding pressure is profiled in two stages: 75 MPa for the first 2.5 s, then 45 MPa for the gate-seal phase. Injection speed is reduced during the final 15 mm of fill to prevent gas entrapment at latch hooks. Regrind ratio is capped at 15% by weight and permitted only in the pin retainer plate, not in the external sealing face. Terminal products include IEC 62196 type-2 inlet housings, DC mid-connector pin retainers and charge-port flap latch mechanisms. Compliance testing follows IEC 62196-1 for creepage after humidity exposure, IEC 60068-2-30 for damp heat cyclic, and UL 94 vertical burn on the thinnest latch wall. The operational limitation is that hydrolysis resistance does not equal hydrolytic immunity; long contact with condensed brine can still produce surface staining and minor swelling, requiring a defined drainage path.
White goods power connectors experience alkaline detergent mist, high humidity and vibration from unbalanced spin cycles. The grade is injection-moulded with mould temperature at 80°C, cycle time between 25 s and 35 s, using a 24-cavity hot-runner tool with conformal cooling around the latch boss. Glass fibre orientation at the weld line is managed by placing the gate at the edge of the terminal shroud; weld-line strength is verified to ISO 527-2 using a weld-line specimen. Regrind ratio of 20% is typical for non-flame-critical appliance covers but is limited to 10% for the terminal housing because regrind reduces glow-wire margin. Terminal products include door-lock connector housings, motor controller terminal brackets and pump power-in connector shrouds. Compliance testing includes IEC 60695-2-12 glow-wire flammability index, IEC 60695-2-13 glow-wire ignition temperature and IEC 60335-1 abnormal operation. The limiting processing window is narrow; melt temperature above 280°C increases volatile outgassing and tool deposition from flame-retardant degradation, while below 250°C incomplete glass wet-out causes cold-flow lines at the gate.
Outdoor photovoltaic junction box bodies, diode holders and inverter cable entry frames are moulded from BF4232HR where dimensional stability under solar load and protection against contact tracking are both required. If the part forms an external lid, the material must be confirmed in a UV-stabilised black formulation; otherwise additional UV screening or a co-moulded gasket seal is required because the PBT matrix undergoes photo-oxidation over multi-year exposure. Processing uses a 25 mm reciprocating screw with 20:1 L/D, melt temperature 250–260°C and mould temperature 100°C; cooling time is set from the wall thickness of the diode heat-sink boss. The 30% glass fibre content controls creep of the terminal clamping plate, but the moulder must select a screw and check ring with hard surfacing because glass fibre wear causes check-ring leakage and shot-weight drift after approximately 300,000 cycles. Regrind ratio should not exceed 15% unless tensile impact after UV and damp heat is re-qualified. Terminal products include PV array junction boxes, inverter DC input housings and DC disconnect partition walls. Compliance is evaluated to IEC 62790 for junction boxes, UL 746C for outdoor polymeric enclosure performance, and UL 94 vertical burn. Published data for this specific grade after 1000 h of 85°C/85% RH damp heat in photovoltaic junction boxes is limited; each tooling set should be validated with production samples because insert moulding of copper conductors can alter local crystallinity.
Circulating pump volutes and impeller shrouds in residential and light commercial hot water systems subject BF4232HR to sustained contact with oxygenated water at 80–95°C. The hydrolysis-stabilised PBT matrix slows molecular-weight loss at the wetted surface, but it does not permit continuous steam service above 120°C. For thick-section volutes, mould temperature is held at 100°C to maximise crystallinity and reduce water absorption at the cut-face. Melt temperature is kept at 250–260°C, and cooling time is calculated from the square of the maximum wall thickness; premature ejection produces sink marks at the volute tongue and dimensional drift after first wet exposure. The 30% glass fibre reinforcement raises resistance to impeller-side wear, but regrind is excluded from pressure-boundary parts unless flexural modulus and weld-line strength are re-qualified to ISO 178 and ISO 527-2. Terminal products include pump volutes, flanges, sensor wells and impeller shrouds. Compliance for electrical pump assemblies follows IEC 60335-2-40 where applicable; material-level verification is performed by comparing flexural strength before and after immersion at 90°C water for 500 h. The operational boundary is exposure to acidic descaling chemicals and chlorinated water at elevated temperature; such media can accelerate surface attack even in hydrolysis-resistant grades.
Competitive Lanxess Pocan® PBT+GF30%-FR-Hydrolytic BF4232HR prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Pocan® BF4232HR is a 30 wt% glass-fibre-reinforced flame-retardant polybutylene terephthalate (PBT) injection moulding compound with hydrolysis-stabilization chemistry. The manufacturer designates the product as PBT+GF30%-FR-Hydrolytic, and the designation identifies the polymer backbone, the 30% glass-fibre mass fraction, the flame-retardant package, and the hydrolytically stabilized formulation. The grade is supplied as pellets for high-volume reciprocating-screw injection moulding. In comparison with unfilled PBT, tensile modulus shifts from approximately 2,600 MPa to a class-typical 9,500–10,500 MPa when measured according to ISO 527-1/-2; elongation at break decreases from approximately 20–25% for unreinforced PBT to roughly 2–3% for the reinforced FR class. These changes are characteristic of discontinuous glass-fibre reinforcement: stiffness and creep resistance increase while ductile strain capacity decreases. The product is intended for applications in which flame retardance, stiffness, dimensional stability, and resistance to hot-humid or water/glycol environments must be combined in a single material. Density, impact, and melt volume-flow rate are lot- and grade-specific; the current technical datasheet and UL yellow card should be referenced for exact values before tool design release.
Polybutylene terephthalate degrades in hot water and humid air by hydrolytic chain scission of the ester linkages along the polymer backbone. The reaction is autocatalytic because each scission event liberates a carboxylic acid end-group, which increases local polarity and accelerates further attack. In non-stabilized PBT GF30 FR, the loss of molecular weight appears macroscopically as surface chalking, brittle failure, and tensile strength decay. In BF4232HR, the stabilization package reduces the concentration of accessible carboxyl end-groups and retards the propagation step, thereby extending the time before substantial property loss occurs.
The hydrolysis reaction is accelerated by free carboxylic acid end-groups; therefore the stabilization package in BF4232HR functions primarily by end-group modification and chain-extension chemistry. This shifts the molecular-weight distribution to maintain a higher fraction of tie molecules between glass fibres during hydrothermal aging. In non-stabilized PBT GF30 FR, chain scission near the fibre-matrix interface allows debonding and microcracking at lower strain; the hydrolytically stabilized grade slows this sequence. The method of evaluation matters: a short-term tensile test after water/glycol immersion may not distinguish HR from non-HR grades because surface attack dominates early exposure. Notched Charpy impact according to ISO 179-1/1eA and tensile strength at break according to ISO 527-2 are more sensitive to bulk molecular-weight reduction.
Hydrolysis-resistant PBT grades are typically compared by exposing machined tensile specimens according to ISO 527-2 to 85 °C and 85% relative humidity for 1,000 h, or by immersion testing in 50:50 water/ethylene glycol at 130 °C for 48–96 h. The relevant output is percentage retention of tensile strength at break and notched Charpy impact according to ISO 179-1/1eA. Published data for the BF4232HR-specific configuration is limited; therefore a direct retention percentage is not provided here. Industrial design verification should always couple material screening data with part-level exposure because moulded-in stress, weld lines, and sharp radii accelerate hydrolytic attack beyond coupon results. Water absorption measurement according to ISO 62 is a necessary but not sufficient screen; it does not capture the location of water uptake or the autocatalytic end-group effect.
The operational boundary is critical: hydrolysis stabilization slows molecular-weight reduction but does not prevent it. Continuous exposure to saturated steam above 121 °C, strongly alkaline coolants with pH greater than 9.5, or hot concentrated acids remains outside the recommended service envelope. For parts that must endure repeated steam sterilisation cycles, a specialty hydrolysis-resistant polyamide or PPSU should be considered, not PBT.
Typical components include engine-compartment sensor housings, high-voltage battery connector bodies, EGR position-sensor enclosures, coolant manifold connectors, and mechatronic housing covers. In these applications, the material is selected when the assembly must satisfy UL 94 V-0 at a wall thickness of 1.5 mm or lower while retaining dimensionally stable contact spacing after exposure to 50:50 water/ethylene glycol at temperatures up to 130 °C. The electrical and dimensional requirements are normally validated by OEM-specific thermal/humidity cycling tests derived from ISO 16750-4. The material's hydrolytic stabilization makes it more suitable than standard PBT GF30 FR grades for connectors mounted on engine blocks, where condensation, thermal shock, and airborne oil mist are present but pH remains near neutral.
Designers should not substitute BF4232HR for PBT grades without reviewing flammability thickness limits. Some flame-retardant PBT formulations achieve V-0 only at 3.0 mm, whereas connector miniaturization often requires V-0 at 0.75–1.5 mm. The grade is appropriate only if the current UL yellow card confirms the required thickness. Glass-fibre length distribution, weld-line placement, and gate freeze time are part-design variables that affect mechanical and flame-retardant performance in ways that raw material datasheets do not capture.
In high-voltage connector housings, comparative tracking index and surface resistivity after humid aging may be part of the material approval. Those values are available in the manufacturer's electrical property table and must be verified according to IEC 60112 for comparative tracking index and IEC 62631-3-2 for volume resistivity. The hydrolytic HR package can influence surface salt formation after water/glycol splashing, so connector engineers often specify a sealed connector-body design rather than relying on the polymer alone. Terminal retention force after heat-humidity cycles is evaluated on insert-moulded specimens; the material contribution cannot be decoupled from terminal geometry. For e-mobility, the material may be specified in battery-housing vent valves, interlock connectors, and cell monitoring units where chemical exposure is limited to near-neutral cooling fluids and condensation. The material is not recommended for direct contact with strongly alkaline battery electrolytes or hot concentrated acids.
Pre-drying is mandatory before melt processing. A closed-loop desiccant dryer with a dew point below -30 °C and an air temperature of 120 °C for 4 h is used to reduce residual moisture to below 0.02 wt%. At ambient relative humidity above 60% RH, hopper dryers without desiccant beds may not maintain dry feedstock, and moulded parts can show silver streaks, surface splay, and reduced mechanical properties. The melt-temperature window is 250–270 °C; melt temperatures above 280 °C increase the risk of polymer degradation and flame-retardant decomposition. Residence time in the barrel should be kept below 8 min in production; hot-runner drops should be designed without dead spots to prevent accumulation of degraded material.
Mould temperature is held between 80 °C and 100 °C to develop sufficient crystallinity and minimize post-mould shrinkage in humid service. Lower mould temperatures below 60 °C quench the surface and can produce a less crystalline skin, which may slightly increase moisture absorption and reduce hydrolysis resistance. General-purpose thermoplastic injection moulding screws with 20:1 to 25:1 L/D, compression ratios of 2.0:1 to 2.5:1, and free-flow non-return valves are commonly used. Because glass fibre is abrasive, nitrided or bimetallic screw and barrel surfaces are used in extended campaigns. Backpressure in the hydraulic circuit is typically started at 30–60 bar; high backpressure raises melt temperature and increases fibre fracture without improving dispersion enough to justify the property loss.
Venting is more critical than for unreinforced PBT because glass-filled FR compounds can produce volatiles from moisture and additive decomposition. Vent depths of 0.02–0.05 mm are typical for this material class; insufficient venting causes burn marks and mould deposit. Mould steel selection should account for the mildly abrasive nature of glass reinforcement; hardened tool steels or protective coatings on gates, runners, and cavities are used in production runs exceeding 100,000 cycles. Hot-runner systems with externally heated manifolds and thermal gating are used for multi-cavity connector housings; internal hot-runner dead spots degrade material and should be eliminated by free-flow design. The transition from screw plasticizing to injection should use a low-back-pressure profile with decompression limited to 2–3 mm to prevent air entrapment and melt splatter; excessive decompression pulls hot air and degrades the flame-retardant package.
The melt volume-flow rate for the material class is commonly measured at 260 °C with 2.16 kg load according to ISO 1133-1; published values for the specific BF4232HR grade should be obtained from the datasheet before designing long-flow thin-wall tools. Fibre orientation and resulting shrinkage are measured according to ISO 2577 or ISO 294-4. Typical moulding shrinkage for a 30 wt% glass-filled PBT FR grade is on the order of 0.2–0.4% in the flow direction and 0.6–0.9% transverse to flow; exact values depend on gate type, part thickness, and melt-temperature history.
The principal difference between BF4232HR and a non-hydrolysis-stabilized PBT GF30 FR compound is the retention of mechanical properties after hot-water or water/glycol exposure. Standard PBT GF30 FR grades may undergo embrittlement after 1,000 h at 85 °C/85% RH, whereas hydrolysis-stabilized grades such as BF4232HR are formulated to maintain a higher fraction of initial tensile strength under the same exposure. The exact retention advantage is grade-specific and should be confirmed by comparative testing using ISO 527-2 tensile bars and notched Charpy specimens per ISO 179-1/1eA. The HR grade does not usually require a different mould temperature or dryer setup than a standard PBT GF30 FR; the processing window is broadly similar, but the molecular-weight protection changes the acceptable moisture limit and hot-runner residence-time sensitivity.
Compared with unfilled PBT, the grade exhibits higher stiffness and lower elongation, as previously described. Compared with 20 wt% glass-fibre FR PBT, BF4232HR provides higher modulus and better dimensional stability but may show greater warpage anisotropy due to the higher fibre concentration. Compared with 40 wt% glass-fibre FR PBT, BF4232HR usually offers lower melt flow and lower modulus but also reduced tool wear and better weld-line appearance. These differences are orientation-dependent and should be evaluated by mould-flow simulation using measured fibre length distribution, not by datasheet comparison alone.
Another distinction from conventional PBT GF30 FR appears in long-term thermal ageing. The hydrolysis stabilizer may slightly shift the melt behaviour or alter the yellowness index; however the dominant selection variable is weight loss and tensile retention after hot-wet exposure. The HR grade is not a different polymer class; it remains PBT with a 225 °C melting temperature by ISO 11357-1/-3, and the crystalline morphology is responsible for the 200–210 °C heat deflection temperature at 1.8 MPa by ISO 75-1/-2. The long-term thermal ageing boundary is defined by the UL relative thermal index in the current yellow card, not by the melting point or heat deflection temperature alone. Electrical RTI for glass-reinforced PBT FR grades is often in the 130–140 °C range, but the specific BF4232HR listing should be confirmed before assigning continuous-use temperature.
| Requirement | Standard | Typical test condition/class value |
|---|---|---|
| Flammability classification | UL 94 / IEC 60695-11-10 | V-0 at 1.5 mm; confirm current yellow card |
| Tensile modulus | ISO 527-1/-2 | ≈10,000 MPa for PBT GF30 FR class |
| Charpy notched impact | ISO 179-1/1eA | 8–10 kJ/m² at 23 °C for reinforced FR class |
| Heat deflection temperature | ISO 75-1/-2 | 200–210 °C at 1.8 MPa |
| Melt volume-flow rate | ISO 1133-1 | 10–20 cm³/10 min at 260 °C/2.16 kg class range |
| Residual moisture before moulding | Karl Fischer titration | <0.02 wt% |
Validation for connector and sensor housings should include thermal shock from −40 °C to 140 °C under ISO 16750-4 profiles, combined with biased humidity and electrical load. Moulded-in residual stress near metal inserts and screw bosses is a stronger predictor of field cracking than coupon-level retention. The hydrolytic stabilization package in BF4232HR is therefore part of a broader material-specification strategy: pre-drying, mould temperature, venting, and part design all determine whether the stabilization benefit appears in the finished component. The material is not recommended for continuous immersion in boiling aqueous salt solutions, hot alkaline cleaners above pH 9.5, or direct contact with aromatic solvents; chemical resistance data for specific media should be obtained before application release.