| HS Code | 678457 |
| Polymer Type | PBT |
| Ul94 Rating | HB |
| Processing Method | Injection molding |
| Melt Temperature C | 250-270 |
| Mold Temperature C | 80-100 |
As an accredited Lanxess Pocan® PBT+GF20% B3225 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Lanxess Pocan® PBT+GF20% B3225 is packaged in 25 kg moisture-barrier bags, 40 bags per pallet (1,000 kg). |
| Container Loading (20′ FCL) | 20′ FCL container loaded with Lanxess Pocan® PBT+GF20% B3225, packed in 25 kg bags on pallets, secured for ocean freight. |
| Shipping | Lanxess Pocan® PBT+GF20% B3225 is typically supplied as non-hazardous, glass-fiber-reinforced PBT thermoplastic pellets. Ship in moisture-proof, sealed bags or containers, protected from heat, moisture, direct sunlight, and contamination. Normally not classified as dangerous goods; follow local transport regulations and the SDS. |
| Storage | Store Lanxess Pocan® PBT+GF20% B3225 in a cool, dry, well-ventilated area away from direct sunlight, heat, moisture, and strong oxidizers. Keep original packaging sealed and intact, protect from dust and contamination, and follow manufacturer temperature recommendations. Use oldest stock first; avoid open flames and excessive static buildup. |
| Shelf Life | Recommended shelf life is typically 12 months when stored dry, unopened, at room temperature, away from moisture and direct sunlight. |
For under-bonnet connector production, Pocan B3225 is processed on injection molding machines in the 80 t to 120 t clamp force range with a general-purpose screw of 30 mm to 35 mm diameter and L/D 22:1. Drying is mandatory in a desiccant-bed dryer at 120 °C for 4 h to a residual moisture below 0.02 wt%; moisture above this threshold produces silver streaking at the gate and loss of surface gloss on latch arms. Melt temperature is held at 260 °C ± 5 °C, and mold temperature is maintained between 80 °C and 100 °C. In production-scale tooling, glass-fibre orientation gradients through latch cross-sections cause differential longitudinal shrinkage of 0.4% to 0.8%, depending on gate location; this is controlled by placing the gate at the thickest boss and holding packing pressure at 700 bar to 900 bar for 3 s to 5 s. Regrind content is normally limited to 15 wt% after screen sieving at 0.5 mm aperture, because fibre length attrition during regranulation reduces notched Charpy impact. Color masterbatch addition is 1.0 wt% to 2.0 wt%, and an oxidation-stable heat-stabilizer masterbatch is added at 1.0 wt% to 1.5 wt% only where continuous under-bonnet air temperature exceeds 130 °C. The automotive qualification framework is USCAR-2 for electrical connector systems, with thermal cycling validated under ISO 16750-4 and thermal shock under IEC 60068-2-14 Test Na. Flame classification is typically UL 94 HB at 0.75 mm; when a V-0 rating is required, B3225 is not used and a flame-retarded PBT variant is substituted. Terminal product types include engine control unit connector housings, camshaft and crankshaft sensor enclosures, throttle body sensor covers, and relay sockets mounted on firewall brackets.
Low-voltage switchgear terminal blocks molded from B3225 are evaluated primarily against IEC 60947-7-1 for terminal blocks in distribution boards and UL 1059 for North American listed terminal blocks. The polymer must retain adequate comparative tracking index after glass fibres migrate to the surface during high-shear mold filling. Surface fibre content alters IEC 60112:2020 tracking performance, so external lubricants or mold-release agents are excluded; black masterbatch is added at 0.5 wt% to 1.0 wt%, and regrind is rationed at 10 wt% maximum because repeated heat history deepens surface fibre orientation and shrinks creepage-path reliability. Insert molding of brass screws and current bars requires preheating the metal inserts to 110 °C ± 10 °C. Mold temperature is held at 60 °C to 80 °C to limit post-mold shrinkage around the insert, while melt temperature is maintained at 255 °C to 265 °C. Injection speed is kept moderate at 80 mm/s to 120 mm/s to suppress jetting at the metal-polymer interface. Packing pressure is applied at 500 bar to 700 bar for 4 s to 6 s. Production experience shows that microcracking at the insert interface starts when mold temperature falls below 60 °C, driven by differential thermal contraction between brass and PBT. Terminal products include DIN rail terminal blocks up to 1000 V insulation voltage, relay bases, fuse holders, and PCB terminal supports used in industrial control panels.
| Application segment | Compliance standards | Key test method | Typical condition |
|---|---|---|---|
| Automotive connectors and sensor housings | USCAR-2, ISO 16750-4, IEC 60068-2-14, UL 94 HB | Thermal shock, heat aging, flame classification | 0.75 mm wall, 130 °C peak |
| Low-voltage terminal blocks | IEC 60947-7-1, UL 1059, IEC 60112:2020 | Comparative tracking index, insert retention | Brass insert at 110 °C preheat |
| Power tool motor and gear housings | IEC 62841-1, UL 94 HB | Mechanical impact, flame classification | 0.75 mm wall |
| Condensing dryer fan wheels and impellers | IEC 60335-1, IEC 60335-2-11, ISO 2578 | Thermal aging in wet air, end-product endurance | Wet air 50 °C to 60 °C max |
| Lamp holders | IEC 60238:2016, UL 496, IEC 60695-2-11 | Glow-wire, thread dimensional retention | Glow-wire limit 650 °C |
| HVAC actuator housings | UL 60730-1, IEC 61010-1, UL 94 HB | Fire-safety, insulation coordination | 0.75 mm wall |
Across power-tool armature housings, impact loading at low temperatures drives part consolidation and ribbing strategies that reduce secondary assembly. B3225 is processed in multi-cavity cold-runner tools with a melt temperature of 265 °C to 275 °C and a mold temperature of 90 °C to 100 °C; the higher mold temperature promotes fibre wet-out and reduces exposed glass at the surface, which is linked to abrasive wear on ejector pins and slide cores. Regrind is capped at 20 wt% for non-cosmetic internal surfaces, and colour masterbatch is introduced at 2.0 wt% to 3.0 wt%. Because the 20 wt% glass reinforcement raises melt viscosity, back pressure is maintained at 30 bar to 60 bar, and screw decompression is set at 3 mm to 5 mm after plastication to prevent nozzle drool. Venting depth is limited to 0.02 mm to avoid flash while releasing pyrolysis gases from PBT ester bonds at the upper melt-temperature limit. Impact resistance is tested according to IEC 62841-1 for hand-held motor-operated electric tools, and flame classification is UL 94 HB at 0.75 mm. Production-scale failures are commonly traced to core-shift in thick bosses around motor bearings, which increases radial run-out after molding; this is corrected by maintaining a minimum boss wall of 3.0 mm and by gating into the boss rather than adjacent thin walls. Terminal products include angle grinder end caps, drill housing gear covers, blower motor housings, and oscillating multi-tool chassis.
Condensing tumble dryer fan wheels and condensate pump impellers impose simultaneous thermal loading and intermittent aqueous contact. B3225 carries the base 20 wt% glass reinforcement and is not intrinsically hydrolysis-resistant; production practice therefore limits continuous water exposure to 50 °C to 60 °C maximum, and prolonged service above 65 °C in wet air is an operational boundary. A hydrolysis-stabilizer masterbatch is compounded in at 1.0 wt% to 2.0 wt%, and regrind is restricted to 10 wt% because hydrolytically degraded surface layers in recycled material accelerate ester-bond cleavage. Drying at 120 °C for 4 h to 6 h is required; residual moisture above 0.02 wt% is not acceptable because water reacts with PBT ester groups during plasticating and reduces intrinsic viscosity within the barrel. Molding temperatures are held at the lower end of the window, with melt at 250 °C to 260 °C and mold at 70 °C to 80 °C, to limit thermal oxidation. The fan wheel hub contains a convergent weld line; mold trials with valve gates and sequential injection demonstrate that weld-line strength in the hub is highly dependent on melt temperature and drops significantly when barrel residence time exceeds 8 min at 260 °C. Ester hydrolysis in neutral condensate follows pseudo-first-order kinetics with respect to available water concentration, but published data for this specific configuration is limited; end-of-life burst-speed testing on molded fan wheels is therefore the controlling validation method. Compliance is tested under IEC 60335-1 and the relevant part IEC 60335-2-11 for tumble dryers, with material aging evaluated by ISO 2578 or internal end-product endurance protocols. Terminal products include condenser fan wheels, condensate pump impellers, water-distribution inserts, and humidity-sensor mounting brackets.
Dimensional control in E14/E27 lampholder production is governed by thread tolerance retention after repeated thermal cycling from lamp-startup temperatures. B3225 is used when the holder is not directly exposed to UV-rich light and when glow-wire requirements are limited to 650 °C or below; if IEC 60695-2-11 glow-wire testing at 850 °C is mandated, the grade is typically excluded. A titanium dioxide whitening masterbatch is added at 1.0 wt% to 2.0 wt%, and regrind is limited to 15 wt%. Brass contact pins are preheated to 90 °C to 110 °C before insert molding; mold temperature is held at 70 °C to 90 °C to balance thread gloss and post-shrinkage. Lampholder threads are produced with core-side cooling and ejection delay to stabilize the pitch diameter; post-mold shrinkage of 0.5% to 0.8% must be absorbed in the tool design. The governing standards are IEC 60238:2016 for lampholders and UL 496 for North American lampholders. Terminal products include E14 and E27 lamp sockets, GU10 bases, integrated LED lamp housings, and screw-thread adapters for decorative luminaires.
Building-automation HVAC damper and valve actuators use B3225 for structural housings that must survive gear-train reaction loads and fire-safety class evaluations. Compliance draws from UL 60730-1 for automatic electrical controls and IEC 61010-1 where control-gear insulation coordination is relevant. Flame classification is UL 94 HB at 0.75 mm; external HV bus-bar applications requiring V-0 are not serviced by this grade. Rib-to-wall thickness ratio is kept between 0.5 and 0.7 to prevent reverse-side sink over gear-bearing seats, and the tool is gated into the thickest boss with a valve-gated hot runner to avoid flow hesitation behind thin ribs. Melt temperature is maintained at 255 °C to 265 °C, mold temperature at 80 °C to 90 °C, and fill speed at 150 mm/s to 200 mm/s. Regrind is permissible up to 20 wt%, carbon black UV masterbatch at 0.5 wt% to 1.0 wt% is used only with black housings, and no internal lubricant is incorporated because gear-grease compatibility testing requires absence of silicone migration. Production-scale failure data indicate that warpage across motor-bearing saddles increases when cavity-to-core temperature difference exceeds 10 °C; active mold-temperature control with separate core and cavity circuits is therefore used. Terminal products include damper actuator housings, valve actuator gear covers, thermostat bases, and duct-sensor mounting brackets.
Competitive Lanxess Pocan® PBT+GF20% B3225 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
The Lanxess Pocan® B3225 product is a pelletized short-glass-fiber-reinforced polybutylene terephthalate (PBT) compound with a nominal glass-fiber loading of 20 wt%. Under ISO 1043-1, the material is designated PBT-GF20. The B3225 grade is differentiated from unfilled PBT grades by higher stiffness, heat deflection temperature, and dimensional stability, and from PBT-GF30 grades by lower melt viscosity, lower density, and generally better thin-wall flow. Density determined by ISO 1183-1 is typically near 1.45 g/cm³. Tensile mechanical values are measured on type 1A specimens conditioned at 23 °C and 50% relative humidity under ISO 527-1/-2. A representative tensile modulus close to 7000 MPa and tensile stress at break near 115 MPa are published for this grade. Elongation at break normally falls in the region of 3% to 4%, which makes the compound stiffness-critical in design and restricts permissible snap-fit strain unless geometry is recalculated.
Charpy notched impact measured according to ISO 179-1/1eA at 23 °C is typically near 8 kJ/m². The heat deflection temperature under 1.8 MPa load by ISO 75-1/-2 is reported near 200 °C, while unfilled PBT typically remains below 65 °C in the same test. Table 1 compares representative supplier-published values across glass contents. The data are typical values, not specification limits, and current datasheets govern for production release.
| Property | Test standard | Pocan B3225 PBT+GF20% | Unfilled PBT | PBT+GF30% |
|---|---|---|---|---|
| Density at 23 °C | ISO 1183-1 | 1.45 g/cm³ | 1.30 g/cm³ | 1.55 g/cm³ |
| Tensile modulus | ISO 527-1/-2 | 7000 MPa | 2600 MPa | 10000 MPa |
| Tensile stress at break | ISO 527-1/-2 | 115 MPa | 55 MPa | 135 MPa |
| Charpy notched impact at 23 °C | ISO 179-1/1eA | 8 kJ/m² | 4 kJ/m² | 10 kJ/m² |
| HDT/A at 1.8 MPa | ISO 75-1/-2 | 200 °C | 60 °C | 210 °C |
The key design consequence of the 20 wt% fiber loading is anisotropy. Fiber orientation in the flow direction raises modulus and reduces linear thermal expansion, but transverse properties remain closer to matrix behavior. Coefficients of linear thermal expansion measured under ISO 11359-2 for glass-reinforced PBT fall in the range of 0.2 × 10⁻⁴ K⁻¹ to 0.4 × 10⁻⁴ K⁻¹ in the flow direction and can be roughly twice that transverse to flow. Mold shrinkage is similarly direction-dependent; a flat plate tool may record 0.4% to 0.6% parallel to flow and 0.8% to 1.2% transverse to flow, depending on gate location, packing pressure, and part thickness. These differences from unfilled PBT require revised mold-dimension allowances and gate placement; otherwise, corner warpage in housings can exceed design tolerance.
Before melt processing, the glass-reinforced PBT pellets must be dried to remove moisture that otherwise hydrolyzes the ester backbone during barrel residence. A desiccant dryer set to 120 °C for 4 h to 6 h is typical; the drying-air dew point should be below -30 °C, and residual moisture should not exceed 0.03% before molding. Incoming moisture can be determined by ISO 15512 or equivalent Karl Fischer methods. On production-scale reciprocating-screw injection machines, the melt temperature is maintained between 250 °C and 270 °C. A melt temperature below 250 °C increases injection pressure and can produce flow lines and poor glass-fiber dispersion at the melt front; a melt temperature above 270 °C shortens the decomposition time and produces yellowing, viscosity loss, and impact reduction. Cumulative barrel residence time should be kept below 10 min; any machine interruption should be followed by purging with a fresh PBT grade before restarting production.
Mold temperature is usually controlled between 60 °C and 100 °C. The lower limit may be sufficient for nonstructural clips, but mold temperatures below 60 °C freeze the skin layer before crystallization completes and can create visible jetting, weld-line weakness, and lower adhesion to inserts. Higher mold temperatures near 100 °C improve surface gloss and crystallization but extend cycle time and can increase shrinkage differentials. The glass fibers in B3225 raise melt viscosity relative to unfilled PBT; injection pressure should be adjusted on the basis of actual melt-front area rather than material cost. Holding pressure on hydraulic machines with an intensification ratio near 10:1 commonly falls in the 50 MPa to 100 MPa range, but cavity-specific pressure measurement is more reliable than machine pressure setpoints.
A general-purpose three-zone screw with L/D of 20:1 to 25:1 and a compression ratio from 2:1 to 3:1 is adequate for many applications; barrier screws may reduce glass-fiber attrition and improve mixing. Back pressure should be kept above 30 bar for homogenization but below 100 bar to limit fiber breakage. Gate diameter should not be smaller than 0.8 mm in high-cavity tools; smaller gates can generate excessive shear heating and resin degradation at the gate land. Hot-runner systems with dead spots should be avoided or validated by short-shot studies because PBT can retain degraded material in stagnant zones. Production-scale molds for connector housings often show that venting depth of 0.02 mm to 0.03 mm at weld lines is required to prevent diesel marks; insufficient venting is a frequent cause of cavity-to-cavity impact inconsistency.
When replacing an unreinforced PBT housing with B3225, the primary mechanical shift is a large increase in tensile modulus and heat deflection temperature, combined with lower elongation at break and higher notch sensitivity. Snap-fit geometry must be recalculated using strain data from ISO 527-2; retaining unreinforced PBT deflections can cause the root section to exceed the lower elongation limit of the glass-filled compound. The allowable undercut depth may need to be reduced by 10% to 20%, or the snap beam length increased, to keep outer-fiber strain below the glass-filled material limit. The higher modulus also raises assembly and retention forces at equal deflection, which must be checked against actuator force and boss capacity.
Compared with PBT+GF30, B3225 has lower stiffness, lower density, and generally easier melt flow in thin-walled sections. The tensile modulus difference is approximately 3000 MPa when moving from 20 wt% to 30 wt% glass. A PBT+GF30 design can carry a higher short-term static load, but is more likely to exhibit glass-fiber surface roughness, orientation-induced warpage, and mold wear. The 20 wt% grade is therefore selected when surface quality or processability outweighs absolute stiffness. When B3225 is compared with a polyamide 66 grade containing 20 wt% glass, the PBT grade absorbs less water and retains dimensions better in humid environments; published saturation water absorption under ISO 62 for PBT-GF20 is often below 0.5%, whereas PA66-GF20 values can exceed 1.0%. The PBT grade also processes at lower melt temperatures than PA66, reducing energy input, but it generally has lower notched impact and lower continuous heat-aging resistance in hot-oil or coolant environments above 100 °C.
Typical application fields for B3225 include electrical and electronic housings, sensor mounts, automotive interior brackets, domestic appliance bases, and power-tool shells where dimensional stability under heat is required. The heat deflection temperature near 200 °C under ISO 75-1/-2 permits short-term exposure to paint-bake cycles or limited soldering environments, provided the peak temperature and time are validated. For electrical insulation parts, dielectric strength is measured by IEC 60243-1 and comparative tracking index by IEC 60112; grade-specific values must be taken from the supplier yellow card rather than generic plastic tables. Flammability classification under UL 94 is thickness- and color-dependent and must be confirmed for the exact part design. Regulatory compliance can be evaluated through supplier declarations against RoHS Directive 2011/65/EU as amended by (EU) 2015/863 and REACH Regulation (EC) No 1907/2006; the grade should not be assumed to satisfy food-contact requirements under EU 10/2011 or FDA 21 CFR 177.1660 unless explicitly declared.
The operational boundary of greatest concern is hydrolysis. PBT ester linkages degrade in hot aqueous media, so continuous exposure to water above 60 °C or saturated steam may reduce molecular weight and notched impact even where room-temperature water absorption is low. Applications such as dishwasher pump bodies, autoclave-sterilized device components, or hot-water plumbing should be accepted only after performing mechanical testing after environmental aging under ISO 527-2 and ISO 179-1/1eA. Outdoor use requires a UV-stabilized variant or validation under ISO 4892-2 accelerated weathering, because standard glass-filled PBT can develop surface chalking and gloss loss with prolonged UV exposure. Adhesive bonding and painting are limited by the high solvent resistance of PBT; surface activation by flame or plasma is often required, and bonded-joint performance should be revalidated on production parts.
Incoming quality control for B3225 can be organized around a small set of standardized measurements. The certificate of analysis should report glass-fiber content or ash residue by ISO 3451-1, melt volume-flow rate by ISO 1133-1, and residual moisture. A lot-to-lot release check on tensile modulus and notched Charpy impact at 23 °C is sufficient in many production sites to detect gross formulation errors; however, this does not replace application-specific qualification for long-term creep or fatigue. Published data for long-term creep and fatigue of this specific B3225 configuration across all temperature and humidity combinations is limited; design for sustained load should use application-specific testing with ISO 899-1 creep protocols.