| HS Code | 480102 |
| Grade | KEPEX® PBT Unfilled 3300C |
| Polymertype | Polybutylene terephthalate (PBT) |
| Fillercontent | 0% (unfilled) |
| Density | 1.44 g/cm³ |
| Meltflowrate | 20 g/10 min |
| Tensilestrength | 55 MPa |
| Elongationatbreak | 3% |
| Flexuralmodulus | 2500 MPa |
| Flexuralstrength | 85 MPa |
| Notchedcharpyimpactstrength | 3 kJ/m² |
| Heatdeflectiontemperatureat0 45mpa | 200 °C |
| Heatdeflectiontemperatureat1 82mpa | 90 °C |
| Vicatsofteningtemperature | 205 °C |
| Meltingpoint | 225 °C |
| Waterabsorption | 0.08% |
| Volumeresistivity | 1E16 Ω·cm |
| Dielectricstrength | 20 kV/mm |
| Dielectricconstant | 3.2 |
| Dissipationfactor | 0.02 |
| Flammability | UL94 V-0 |
| Moldingshrinkage | 1.5-2.0% |
As an accredited Korea Engineering Plastics KEPEX® PBT Unfilled 3300C factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg net moisture-barrier bags on pallets, KEPEX® PBT Unfilled 3300C is supplied for industrial handling and storage. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with KEPEX® PBT Unfilled 3300C in 25 kg bags, palletized, stretch-wrapped, and secured for export shipment. |
| Shipping | Korea Engineering Plastics KEPEX® PBT Unfilled 3300C is shipped as non-hazardous PBT resin pellets in sealed moisture-barrier bags or boxes, palletized. Protect from moisture, heat, and contamination; store dry. Not regulated for transport; follow the SDS and local regulations. |
| Storage | Store KEPEX® PBT Unfilled 3300C in a cool, dry, well-ventilated area, away from direct sunlight, heat sources, and moisture. Keep in original sealed packaging until use; reseal opened bags tightly. Avoid contamination by oils, solvents, or strong odors. Maintain low humidity and dry before processing if exposed to prevent moisture pickup and hydrolytic degradation. |
| Shelf Life | Typical shelf life is 24 months when stored unopened in original packaging under cool, dry conditions, away from moisture and sunlight. |
Competitive Korea Engineering Plastics KEPEX® PBT Unfilled 3300C prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Korea Engineering Plastics KEPEX® PBT Unfilled 3300C is a non-reinforced, non-flame-retarded polybutylene terephthalate injection-molding grade based on the melt polycondensation of 1,4-butanediol with dimethyl terephthalate or terephthalic acid. It is classified as a medium-flow, semi-crystalline thermoplastic polyester for close-tolerance electromechanical components. Unfilled 3300C contains no glass fiber, mineral filler, or halogenated flame-retardant additive; consequently, its rheological response, warpage direction, and surface appearance differ from filled PBT formulations. The mold shrinkage is anisotropic in the flow and cross-flow directions, with values in the range 1.5–2.0 % parallel to flow and 1.2–1.8 % transverse when measured on 60 mm × 60 mm × 2 mm plaques per ISO 294-4. A melting peak near 225 °C is measured by differential scanning calorimetry using ISO 11357-3 at 10 K/min; recrystallization behavior depends on mold temperature and cooling rate. The grade is supplied in pellet form and is intended for reciprocating-screw injection molding. Drying is mandatory before melt processing: pellets exposed to ambient humidity above 60 % RH absorb atmospheric moisture, which causes hydrolytic chain scission during processing and reduces melt viscosity and impact retention. A desiccant-bed or dehumidifying dryer set at 120 °C for 4 h, or 130 °C for 3 h, with a dew point of −30 °C or lower, reduces residual moisture below 0.02 % by weight, as verified by Karl Fischer titration according to ISO 15512. Processing with wet resin routinely produces surface splay and a measurable loss of Charpy notched impact.
Incoming resin lots should be checked for melt volume-flow rate per ISO 1133-1 and moisture content per ISO 15512; lot-to-lot variation above ±5 % in MVR can alter filling pressure in multi-cavity tools. Pre-drying of regrind at the same conditions as virgin pellets is required if regrind has been stored outside a hopper dryer. In high-humidity coastal production environments, hopper residence time beyond 30 min at 90 % RH may reintroduce surface moisture; a nitrogen blanket or sealed hopper with −30 °C dew-point feed air is used. The property envelope in Table 1 is derived from standard test plaques and illustrates unfilled PBT of this medium-flow class. Lot-specific release values are listed in the certificate of analysis and can deviate within normal production tolerance.
For a 30 % glass-fiber-reinforced grade, short-glass reinforcement raises flexural modulus from approximately 2.3 GPa for unfilled 3300C (ISO 178) to 7–10 GPa for the reinforced material, while tensile strain at break falls from approximately 150 % to 2–3 % (ISO 527-2/1A). The heat-deflection temperature under 1.80 MPa shifts from roughly 60 °C for unfilled 3300C (ISO 75-2/A) to above 205 °C when reinforcing with short glass. The differences in anisotropic fiber alignment produce weaker weld-line strength retention in glass-filled PBT; unfilled 3300C retains a higher weld-line impact fraction because no fiber orientation discontinuity exists at the melt front. A flame-retarded UL 94 V-0 grade, whether brominated or phosphorus-containing, may reduce tracking resistance and notched impact relative to unfilled PBT. Unfilled 3300C does not carry a V-0 classification; its flammability rating is typically HB at 0.75 mm and above. The absence of flame-retardant and reinforcing additives improves lot-to-lot color consistency and reduces tool-surface plate-out sometimes observed with certain flame-retardant packages.
Compared with polyamide 66, unfilled 3300C absorbs significantly less moisture. Water absorption at saturation is below 0.5 % by weight, whereas PA66 can absorb 7–9 % at saturation. Consequently, electrical properties and dimensional stability are less influenced by humidity. However, the heat-deflection temperature of unfilled PBT is lower than that of 30 % glass-filled PA66 or PBT; PA66 also has better resistance to some hot lubricants. Compared with polycarbonate, unfilled PBT has lower notched impact and lower optical transparency, but better fatigue and chemical resistance to many automotive fluids.
| Property | Standard and condition | Typical value |
|---|---|---|
| Density | ISO 1183-1, 23 °C | 1.31 g/cm³ |
| Melting temperature | ISO 11357-3, 10 K/min | 225 °C |
| Melt volume-flow rate | ISO 1133-1, 250 °C/2.16 kg | 25 cm³/10 min |
| Mold shrinkage, parallel | ISO 294-4, 60 mm × 60 mm × 2 mm | 1.5–2.0 % |
| Mold shrinkage, transverse | ISO 294-4, 60 mm × 60 mm × 2 mm | 1.2–1.8 % |
| Tensile stress at break | ISO 527-2/1A, 23 °C | 55 MPa |
| Tensile strain at break | ISO 527-2/1A, 23 °C | 150 % |
| Flexural modulus | ISO 178, 23 °C | 2.3 GPa |
| Flexural strength | ISO 178, 23 °C | 80 MPa |
| Charpy notched impact | ISO 179-1/1eA, 23 °C | 4.5 kJ/m² |
| Charpy unnotched impact | ISO 179-1/1eU, 23 °C | No break at 23 °C |
| Heat-deflection temperature | ISO 75-2/A, 1.80 MPa | 60 °C |
| Heat-deflection temperature | ISO 75-2/B, 0.45 MPa | 150 °C |
| Vicat softening temperature | ISO 306, B50 | 170 °C |
| Water absorption, 24 h | ISO 62 | 0.08 % |
| Volume resistivity | IEC 62631-3-1 | 1 × 1015 Ω·m |
| Surface resistivity | IEC 62631-3-2 | 1 × 1014 Ω |
| Dielectric strength, 1.0 mm | IEC 60243-1 | 18 kV/mm |
| Comparative tracking index | IEC 60112, solution A | 600 V |
| UL 94 rating | UL 94 | HB at 0.75 mm |
Applications for unfilled 3300C are based on the combination of moderate heat resistance, dimensional stability after post-mold shrinkage stabilization, and low dielectric loss across a range of frequencies. Candidate modules include bobbins and coil forms in ignition systems, relay housings, terminal strips, circuit-breaker internal components, brush card insulators, and sensor housings where the environmental temperature does not exceed the heat-distortion threshold under load. For relay housings, insulation resistance after damp heat can be measured per IEC 60068-2-78 at 40 °C/93 % RH for 56 days. The material is not specified for continuous hot-water service above 60 °C; hydrolytic aging in aqueous environments above that threshold reduces molecular weight and notched impact. For connector bodies requiring UL 94 V-0 at 0.75 mm, the unfilled HB grade is not acceptable; a flame-retarded PBT or PBT alloy is required. In switchgear applications, creepage and clearance design should follow IEC 60664-1 for pollution degree and overvoltage category.
Chemical resistance is good for aliphatic hydrocarbons, mineral oils, and alcohols at 23 °C; strong acids, strong alkalis, and steam autoclave cycling degrade the polymer. For under-hood components with hot ethylene glycol, long-term exposure data on this specific grade are limited; immersion testing per ASTM D543 or ISO 175 on molded plaques is required. Flexural creep modulus after 1000 h at 60 °C is typically lower than the room-temperature flexural modulus; long-term load-bearing designs should use conservative creep values derived from ISO 899-2.
Machine parameters for a 20:1 to 25:1 L/D general-purpose screw with a compression ratio of 2.0:1 to 2.5:1 and a check-ring tip are appropriate for unfilled PBT. Recommended melt temperature is 230–250 °C; barrel zones should be profiled from 230 °C in the rear zone to 250 °C at the nozzle. Melt temperatures above 260 °C accelerate thermal degradation, generating tetrahydrofuran and discoloration. Mold temperature should be maintained at 60–100 °C to control crystallization rate and reduce post-mold warpage. Injection pressure at transfer is typically 60–100 MPa, with hold pressure 40–60 % of peak injection pressure for gate-seal compensation. Back pressure should be kept at 0.3–0.7 MPa; excessive back pressure raises melt temperature and reduces cycle stability. Screw rotation speed should be 50–150 rpm depending on screw diameter, so that plasticating time does not exceed the cooling timer. Nozzle orifice should be a reverse-taper type to avoid drool, with zone control at ±5 °C. Residence time at 240 °C should not exceed 8–10 min; purging with polypropylene or a commercial purge compound after shutdown prevents black specks from degradation in the hot runner or manifold.
Cavity pressure sensors can detect gate-freeze time; typical gate-seal time for unfilled PBT is 2–4 s for wall thickness 1.5 mm at 80 °C mold temperature. A cushion of 3–6 mm should be maintained at screw retract; excessive decompression draws air into the barrel and causes splay in the next shot. Standard screw decompression is 2–5 mm. Short-shot failures in pin connector molding are observed when the melt front solidifies before filling thin latch features; increasing mold temperature from 60 °C to 80 °C improves fill distance by delaying crystallization. However, mold temperatures above 100 °C may extend cycle time and increase plate-out risk.
Because unfilled PBT is semi-crystalline, shrinkage compensation depends on pack pressure, gate freeze time, and mold temperature. For gear teeth or connector pitch dimensions, tool builders usually apply a shrinkage factor of 0.016–0.020 mm/mm in the flow direction and 0.014–0.018 mm/mm cross-flow. Dimensions are stable after 24 h at 23 °C/50 % RH; post-mold annealing for 2 h at 120 °C can stabilize dimensional changes for service temperatures up to the HDT. If the molding process uses high injection speed above 100 mm/s, jetting and weak weld lines occur in thin sections below 1 mm; gate diameter should be 0.5–0.8 times wall thickness with a land length of 0.5–1.0 mm. For very thin wall sections below 0.8 mm, filling pressure can exceed 120 MPa, causing flash and core pin deflection. In those cases, raise mold temperature to 100 °C and increase melt temperature to 250 °C, but monitor residence time. Regrind use for unfilled PBT at 20–30 % by weight is generally accepted in noncritical electrical applications if the regrind is dry and free of contamination; more than 30 % recycled material often reduces notched Charpy impact by 10–20 % and increases lot-to-lot color variance. For connectors with retained impact requirements, virgin material only is recommended.
The UL 94 classification for unfilled 3300C is HB at 0.75 mm, not V-2 or V-0. Applications requiring self-extinguishing behavior require a listed flame-retarded alternative. The comparative tracking index of unfilled PBT is often 600 V under IEC 60112 solution A, but surface contamination or condensation can reduce tracking resistance in field environments. Dielectric strength of 18 kV/mm at 1 mm (IEC 60243-1) supports low-voltage insulation; safety margins for clearance and creepage still apply per IEC 60664-1. Volume resistivity of 1 × 1015 Ω·m remains relatively insensitive to humidity below 50 % RH, but surface resistivity can drop by one to two decades under condensation; hydrophobic PBT is not a substitute for sealing at IEC 60529 IP67. In alternating-current motor brush-card insulators, the dissipation factor and dielectric constant should be verified at the operating temperature, because service above 120 °C may reduce tensile strength and increase dielectric loss.
For hot-runner tools, the manifold and drop temperatures should not exceed 250 °C. Purge after hot-runner interruptions longer than 10 min with a melt-stable purge compound; degraded PBT residue at the tip can cause intermittent short shots and black speck contamination. In multi-cavity relay housings, cavity-to-cavity filling imbalance above 5 % can be corrected by runner geometry rather than raising melt temperature, which reduces thermal safety margin.
| Regulation or requirement | Status | Verification and scope |
|---|---|---|
| RoHS 2011/65/EU, Annex II | Below maximum concentration values for homogeneous material classes | IEC 62321-5 for Cd, IEC 62321-4 for Hg, IEC 62321-7-2 for Cr(VI), supplier analytical certificates |
| REACH SVHC candidate list | Supplier declaration required for resin supply | REACH Article 33; safety data sheet Section 15 |
| UL listing | HB at 0.75 mm | UL Yellow Card |
| Food-contact status | Not granted for all end uses; migration testing required | 21 CFR 177.1660 applies to resin; final article compliance is independent |
| ISO 9001 manufacturing | Site certification required | Audit certificate |
Storage of unopened bags in ambient conditions below 50 % RH and below 40 °C avoids pre-drying requirements for at least 12 months from the production date. Opened bags should be resealed or transferred to a hopper dryer with desiccant regeneration. For parts exposed to continuous hot-battery acid splash, fluoropolymer or polypropylene grades may be more suitable; PBT is not recommended for strong alkali or hot concentrated acid service.