Korea Engineering Plastics Kepex Pbt Pet Gf45 4345gf

Korea Engineering Plastics KEPEX® PBT+PET+GF45% 4345GF

    • Product Name: Korea Engineering Plastics KEPEX® PBT+PET+GF45% 4345GF
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 168014
    Materialtype PBT/PET alloy
    Reinforcement Glass fiber
    Glassfibercontent 45%
    Density 1.65 g/cm³
    Tensilestrength 140 MPa
    Tensileelongationatbreak 2%
    Flexuralmodulus 10000 MPa
    Flexuralstrength 200 MPa
    Notchedizodimpactstrength 8 kJ/m²
    Heatdeflectiontemperature 210 °C at 1.82 MPa
    Meltingpoint 225 °C
    Waterabsorption 0.05%
    Moldshrinkage 0.2-0.5%
    Flammability HB

    As an accredited Korea Engineering Plastics KEPEX® PBT+PET+GF45% 4345GF factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing KEPEX® PBT+PET+GF45% 4345GF is packaged in 25 kg moisture-resistant bags, supplied on pallets for industrial handling and storage.
    Container Loading (20′ FCL) 20′ FCL loading of Korea Engineering Plastics KEPEX® PBT+PET+GF45% 4345GF in 25 kg bags on pallets, dry container, standard export packing.
    Shipping KEPEX® PBT+PET+GF45% 4345GF is supplied as glass-fiber-reinforced resin pellets in moisture-barrier bags or lined octabins, palletized and stretch-wrapped. Ship in dry, clean, ventilated conditions, away from heat and direct sunlight. Handle as non-hazardous industrial material; label with grade, lot, and weight; follow applicable transport regulations.
    Storage Store in a cool, dry, well-ventilated warehouse away from direct sunlight, heat sources, moisture, and incompatible chemicals. Keep in original, tightly closed containers, palletized off the floor. Avoid dust generation, static buildup, physical damage, and contamination. Follow manufacturer SDS/TDS and local regulations.
    Shelf Life Shelf life is generally indefinite when stored dry, cool, away from direct sunlight, moisture, and contaminants in sealed original packaging.
    Free Quote

    Competitive Korea Engineering Plastics KEPEX® PBT+PET+GF45% 4345GF prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    KEPEX® PBT+PET+GF45% 4345GF is a hybrid semi-crystalline polyester injection-molding compound in which a nominal 45 wt% discontinuous glass-fiber reinforcement is dispersed in a polybutylene terephthalate/polyethylene terephthalate matrix. The suffix “GF45” identifies the glass-fiber loading, while the numeric designation 4345 serves as the product model identifier within the Korea Engineering Plastics KEPEX® portfolio. The material is supplied as free-flowing cylindrical granules, and its polymer base combines the rapid crystallization and melt-flow characteristics of PBT with the higher thermal resistance and lower creep of PET. For incoming resin verification, glass-fiber content may be determined by calcination according to ISO 3451-1:2019, and molded identification is typically marked as >PBT+PET-GF45< under ISO 11469:2016. Density for this class of compound is generally reported between 1.63 g/cm³ and 1.73 g/cm³ by ISO 1183-1:2019, Method A. The grade is not a simple 45% glass-filled PBT or PET; the dual-polyester matrix is formulated to balance processability against dimensional stability. Published data for this specific configuration is limited, and the numerical values provided here represent industrial ranges for equivalent 45 wt% glass-filled PBT/PET blends rather than lot-specific certificate values. The material should not be specified for load-bearing designs without performing lot-specific mechanical testing on molded specimens.

    How Does the 45 wt% Glass-Filled PBT/PET Morphology Influence Load Transfer and Warpage?

    The mechanical response of KEPEX® PBT+PET+GF45% 4345GF is governed not only by the nominal glass-fiber content but also by fiber-length retention during compounding and subsequent injection molding. In a co-rotating twin-screw extruder with 40:1 L/D and glass fiber fed downstream into the melt, number-average fiber length after compounding typically falls between 250 µm and 350 µm for similar grades. Injection molding through a conventional reciprocating screw further reduces fiber length, often to 180 µm to 250 µm, because of fiber-fiber abrasion and fiber-screw metal contact. This fiber attrition suppresses the effective aspect ratio below the value often assumed from virgin chopped strands. A mean fiber aspect ratio above 20 is generally required to transfer tensile stress from the polyester matrix to the glass fiber efficiently; below that threshold, stiffness retention becomes disproportionately sensitive to fiber orientation and weld-line location.

    Orientation gradients across the part thickness create asymmetric shrinkage. The skin layer, where rapid cooling freezes highly oriented fibers, shrinks less in the flow direction, while the slower-cooling core develops transverse orientation and greater through-thickness shrinkage. The resulting differential strain produces out-of-plane warpage in flat parts with wall sections above 3.0 mm. This warpage is not fully eliminated by mold-temperature elevation alone. Production-scale molding of structurally flat housings typically requires gate placement that balances filling vectors, restrictive feed systems, and low-shear screw rotation. High glass-fiber content also reduces melt elasticity at the advancing flow front; weld lines formed downstream of core pins or multi-gate layouts exhibit tensile strength reductions of 30% to 50% relative to non-weld-line material when tested under ISO 527-2:2012. Therefore, structural load paths should be moved away from predicted weld-line regions.

    For mechanical design calculations based on ISO 527-2:2012 and ISO 178:2019, the tensile modulus of a 45 wt% glass-filled PBT/PET compound falls between 14 000 MPa and 16 500 MPa at 23 °C. Flexural strength measured at 23 °C usually lies between 220 MPa and 260 MPa. Charpy notched impact strength under ISO 179-1/1eA:2023 is typically 9 kJ/m² to 13 kJ/m² at 23 °C, with a lower range of 5 kJ/m² to 8 kJ/m² at −30 °C. These values are not isotropic; tensile modulus in the cross-flow direction can be 15% to 25% lower than in the flow direction, depending on gate design and part thickness. Heat deflection temperature under ISO 75-1/2:2020 at 1.8 MPa is generally between 205 °C and 220 °C for specimens molded under recommended conditions. The PET fraction raises the upper end of this range relative to PBT GF30, but only if mold temperature is high enough to permit PET crystallization.

    Processing Envelope and Drying Thresholds for Glass-Filled PBT/PET

    Residual moisture is the principal processing risk for this product class. Both PBT and PET hydrolyze in the melt when moisture exceeds approximately 0.02 wt%. Hydrolytic chain scission reduces melt viscosity, shifts flow-front behavior, degrades weld-line strength, and increases variability in molded-part dimensions. Pre-drying in a desiccant dryer at 120 °C for 4 h to 6 h is the standard threshold, with a dew point of −40 °C or lower. Warehouse-aged granules exposed to ambient humidity above 60% RH may require drying times up to 8 h. Moisture content can be verified by ISO 15512:2016 or by a calibrated Karl Fischer titration. Drying above 140 °C should be avoided because prolonged exposure can oxidatively degrade polyester surfaces and cause yellowing of natural resins.

    Melt temperature measured at the nozzle should be held between 250 °C and 270 °C. Barrel temperature profiles on a conventional three-zone injection barrel are commonly set with the rear zone at 240 °C to 250 °C, the middle zone at 250 °C to 260 °C, and the front zone at 255 °C to 265 °C. Nozzle temperature is set at 260 °C to 270 °C. Above 280 °C, the PET fraction undergoes thermal-oxidative degradation, producing acetaldehyde, gassing, and visible yellowing. Residence time at melt temperature should not exceed 5 min; longer residence generates melt-flow-index drift and splay. If the machine barrel capacity is much larger than shot size, use a shot volume of 50% to 70% of rated barrel capacity to limit residence time. Melt temperature below 250 °C is not advisable because fiber wetting becomes incomplete and melt pressure at the gate rises sharply.

    Mold temperature is a critical threshold between dimensional stability and cycle-time economy. The recommended mold temperature range is 80 °C to 120 °C. Below 70 °C, the PET fraction may fail to crystallize sufficiently, producing a matte or amorphous skin and elevated post-molding shrinkage. Parts molded at cold mold temperatures may shrink an additional 0.1% to 0.2% during subsequent thermal aging. Above 130 °C, cycle time rises without proportional dimensional benefit, and PET thermal degradation at the hot-runner gate becomes more likely. For thin-wall parts below 1.5 mm, use 80 °C to 100 °C mold temperatures to avoid short shots. For thick sections above 3.0 mm, use 100 °C to 120 °C to reduce sink marks and improve flatness.

    Injection pressure for this glass-filled grade is typically 80 MPa to 120 MPa hydraulic pressure, depending on flow length and wall thickness. Holding pressure should be 50% to 70% of peak injection pressure, applied for 2 s to 6 s per millimeter of nominal wall thickness. Back pressure is usually 0.3 MPa to 0.7 MPa, sufficient to homogenize the melt without excessive fiber damage. Screw rotation speed should remain between 60 rpm and 120 rpm. High back pressure above 1.0 MPa accelerates fiber attrition and increases melt temperature without improving dispersion. Screw and barrel wear protection is necessary because dispersed glass fibers abrade nitrided surfaces; bimetallic barrels and hard-chrome or nickel-based screw coatings are commonly used on production equipment. Vented barrels are generally avoided for glass-filled polyester because fiber can accumulate at the vent and cause degradation.

    Hot-runner systems require low-shear channel geometry and no dead zones. Manifold temperatures should be held at 255 °C to 265 °C, and gate tips should be heated independently where possible. Flow channels below 2.0 mm diameter are not recommended because glass-fiber bundles can bridge at sharp bends. Valve-gated hot runners are preferred over thermal sprue gates for high-glass-fiber compounds because they permit cleaner gate freeze-off. Vent depth in the mold cavity is typically 0.02 mm to 0.03 mm for glass-filled polyester. Insufficient venting causes burn marks and gas traps at the end of fill, while excessively deep vents create flash. For semi-crystalline glass-filled compounds, cold-runner molds with full-round runners of 4.0 mm to 6.0 mm diameter and short runner lengths generally reduce pressure loss and improve fiber-length retention.

    Processing parameter window for KEPEX® PBT+PET+GF45% 4345GF
    ParameterRecommended rangeControl point
    Moisture before molding<0.02 wt%ISO 15512:2016 or Karl Fischer
    Pre-drying temperature120 °CDesiccant dryer, dew point −40 °C
    Pre-drying time4 h to 6 hUp to 8 h if stored above 60% RH
    Melt temperature at nozzle250 °C to 270 °CNozzle thermocouple
    Maximum melt temperature<280 °CDo not exceed for more than 5 min
    Mold temperature80 °C to 120 °CThin walls 80–100 °C; thick walls 100–120 °C
    Injection pressure80 MPa to 120 MPaHydraulic pressure at screw tip
    Holding pressure50–70% of peakApplied 2–6 s per mm wall
    Back pressure0.3 MPa to 0.7 MPaAvoid above 1.0 MPa
    Screw speed60 rpm to 120 rpmReciprocating screw
    Hot runner manifold255 °C to 265 °CChannel diameter ≥ 2.0 mm

    At the compounding stage, side-fed glass fiber is preferred over fiber addition at the main feed throat. Feeding chopped glass at the first barrel section increases fiber attrition because the solid fibers travel through the entire melting zone. Side feeding into the melt reduces uncontrolled fiber breakage and helps maintain the target fiber-length distribution. Compounding of PBT/PET glass-filled grades is generally performed on co-rotating twin-screw extruders with 40:1 L/D to 44:1 L/D and vacuum venting after the side-feed port. The screw profile typically includes a melting section before the feed port, a distributive mixing section after the feed port, and a low-shear venting section. Too many kneading blocks after glass addition reduce fiber length and lower tensile modulus. Too few mixing elements cause glass clustering and poor surface quality. This balance is a known batch-to-batch variation source in industrial compounding.

    When 4345GF Is Substituted for PBT GF30 or PET GF45 in Structural Housings

    KEPEX® PBT+PET+GF45% 4345GF occupies a stiffness class between PBT GF30 and PET GF45, but its processing behavior is closer to that of PBT. Compared with PBT GF30, the 45 wt% glass-filled PBT/PET blend increases tensile modulus by approximately 50% to 70% and raises heat deflection temperature by 10 °C to 20 °C. The penalty appears in melt flow length and impact. The higher glass content lowers spiral flow length under the same injection pressure, and gate pressure must be raised or wall thickness increased to fill the same part geometry. Notched Charpy impact of PBT/PET GF45 is often similar to or only slightly higher than PBT GF30 because the additional glass raises crack propagation through the fiber-matrix interface. PBT GF30 remains preferable where thin-wall filling, low-pressure molding, or lower density are design constraints.

    Compared with PET GF45, the PBT/PET matrix allows lower mold temperatures. Straight PET GF45 usually requires mold temperatures of 120 °C to 140 °C to develop full crystallinity and dimensional stability. The PBT fraction in KEPEX® 4345GF shortens the crystallization half-time and permits molding at 80 °C to 120 °C. This reduces cycle time and tooling heating load. The PET fraction, however, contributes higher surface gloss and improved surface hardness relative to PBT GF30. Compared with PET GF45, the blend may show slightly lower peak HDT and slightly higher creep in hot, dry conditions because the PBT fraction softens earlier. The blend is therefore specified when the application requires PET-like dimensional stability but cannot tolerate the high mold temperatures or slow crystallization of straight PET GF45.

    Relative to PA66 GF50, the 45% glass-filled PBT/PET compound has lower moisture absorption and better dimensional consistency in humid environments. Water uptake after 24 h immersion at 23 °C under ISO 62:2008 is generally below 0.3 wt% for PBT/PET grades, compared with 0.7 wt% to 1.0 wt% for glass-filled PA66. In dry-as-molded conditions, PA66 GF50 typically shows higher tensile strength and higher HDT, but its properties shift more when moisture equilibrates. The polyester grade is therefore selected for electrical housings, sensor brackets, and underhood components where dimensions must remain stable from dry winter air to high summer humidity. However, PBT/PET grades are not recommended for continuous hot-water contact above 80 °C unless a hydrolysis-stabilized additive system is specified; polyester chain scission under aqueous heat can reduce tensile strength by 20% to 40% after extended exposure, depending on temperature and pH.

    In applications such as automotive ignition coil bobbins, ECU housings, wiper motor frames, pump bases, and industrial relay carriers, the selection of KEPEX® PBT+PET+GF45% 4345GF is driven by stiffness, heat resistance, and low moisture sensitivity. Injection molders must plan for higher clamp force than PBT GF30 because glass-filled compounds at 45 wt% load generate higher injection pressure. Clamp force is typically estimated at 0.6 ton/cm² to 0.8 ton/cm² of projected area for parts with 1.5 mm to 3.0 mm wall thickness. Chemical compatibility must also be reviewed. The polyester matrix is sensitive to strong alkaline media and to hot aqueous environments. Amine-based additives and alkaline processing aids should be avoided because they can accelerate polyester chain scission. Mold-release selection should be limited to neutral or slightly acidic specialty agents validated for PBT/PET. Recycled in-plant regrind may be used at up to 20 wt% without loss of specified tensile modulus when the regrind is dry and free of contamination; higher regrind fractions may reduce Charpy impact because glass fiber length is further degraded.

    Comparative typical property ranges for glass-reinforced polyester classes
    PropertyTest standardPBT/PET GF45 classPBT GF30PET GF45
    DensityISO 1183-1:20191.63–1.73 g/cm³1.50–1.56 g/cm³1.66–1.75 g/cm³
    Tensile strength at breakISO 527-2:2012150–180 MPa120–140 MPa160–190 MPa
    Tensile modulusISO 527-2:201214 000–16 500 MPa9 000–10 500 MPa15 000–17 500 MPa
    Flexural strengthISO 178:2019220–260 MPa190–220 MPa230–270 MPa
    Flexural modulusISO 178:201913 000–15 000 MPa8 000–9 500 MPa13 000–16 000 MPa
    Charpy notched impact, 23 °CISO 179-1/1eA:20239–13 kJ/m²8–11 kJ/m²10–14 kJ/m²
    HDT-A 1.8 MPaISO 75-1/2:2020205–220 °C195–205 °C220–235 °C
    Water absorption, 24 h at 23 °CISO 62:20080.1–0.3 wt%0.1–0.2 wt%0.1–0.3 wt%

    Dimensional stability after molding must be verified by measurement of total post-shrinkage. For a 45 wt% glass-filled PBT/PET part molded under the recommended temperature window, total shrinkage from mold to 48 h aging at 23 °C is typically 0.2% to 0.5% in the flow direction and 0.5% to 1.0% in the cross-flow direction. Post-shrinkage after thermal cycling to 150 °C may reach an additional 0.1% to 0.2%, especially if the PET fraction was not fully crystallized during molding. Tolerances below ±0.05 mm on unfixtured dimensions across a 100 mm span are generally not practical for this material without annealing or internal stress relaxation. For flame-retardant or UV-stabilized versions, the property range can shift depending on the additive package; the designation KEPEX® PBT+PET+GF45% 4345GF itself does not imply a specific flame-retardant rating. A UL 94 rating must be confirmed on the final compound and color, and HB at 0.8 mm is the common baseline for non-flame-retardant glass-filled polyester grades, not a certified value for all production lots. Regulatory declarations for REACH, RoHS Directive 2011/65/EU Annex II, and UL 746 component recognition must be obtained from the current lot-specific technical data sheet and compliance certificate. Final part validation for underhood or electrical applications requires testing under the OEM-specific thermal cycling, humidity aging, and mechanical load profile. No single-point thermal or tensile value substitutes for that system-level verification when the part is exposed to simultaneous temperature, vibration, and retained moisture.