Korea Engineering Plastics Kepex Pbt Gf15 Fr Uv 3315gvu

Korea Engineering Plastics KEPEX® PBT+GF15%-FR UV 3315GVU

    • Product Name: Korea Engineering Plastics KEPEX® PBT+GF15%-FR UV 3315GVU
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 803805
    Base Polymer Polybutylene terephthalate (PBT)
    Glass Fiber Content 15%
    Flame Retardancy Flame retardant
    Uv Stabilization UV stabilized
    Density approx. 1.50-1.55 g/cm3
    Tensile Strength approx. 90-100 MPa
    Elongation At Break approx. 2-3%
    Flexural Modulus approx. 5500-6500 MPa
    Notched Izod Impact Strength approx. 5-7 kJ/m2
    Hdt At 1 82 Mpa approx. 195-205 deg C
    Ul 94 Flammability Rating V-0 (typical)
    Water Absorption approx. 0.06-0.08%
    Molding Shrinkage approx. 0.3-0.7%
    Melting Point approx. 225 deg C

    As an accredited Korea Engineering Plastics KEPEX® PBT+GF15%-FR UV 3315GVU factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Packaged in 25 kg moisture-resistant paper bags, 40 bags per pallet, totaling 1,000 kg per pallet for shipment and storage.
    Container Loading (20′ FCL) 20′ FCL container loading with palletized bags of KEPEX® PBT+GF15%-FR UV 3315GVU, moisture-protected and securely stowed for transport.
    Shipping KEPEX® PBT+GF15%-FR UV 3315GVU is shipped as non-hazardous thermoplastic pellets in sealed moisture-barrier bags or containers, palletized and protected from heat, moisture, and UV. Transport per SDS; no UN dangerous-goods classification is indicated unless otherwise stated. Handle in a dry, ventilated area and label with product and batch details.
    Storage Store KEPEX® PBT+GF15%-FR UV 3315GVU in a cool, dry, well-ventilated area, away from direct sunlight, UV exposure, heat, moisture, and ignition sources. Keep in original sealed packaging, on pallets off the floor, and protect from tearing or contamination. Avoid prolonged outdoor storage; rotate stock, do not stack excessively, and follow the SDS.
    Shelf Life Shelf life is typically 12 months in original unopened packaging, stored dry, cool, and protected from direct sunlight.
    Free Quote

    Competitive Korea Engineering Plastics KEPEX® PBT+GF15%-FR UV 3315GVU prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    The KEPEX® PBT+GF15%-FR UV 3315GVU from Korea Engineering Plastics is a polybutylene terephthalate compound in which short glass fibre is incorporated at a nominal 15% weight fraction, together with a flame-retardant package and a UV stabilisation system. The PBT matrix typically exhibits a melting endotherm at 223–225°C and a glass transition at 45–60°C by ISO 11357-3; these values are matrix-class data and do not replace the 3315GVU certificate. The grade identifier 3315GVU separates the material from standard PBT grades by combining a 15% fibre content, an FR rating suitable for thin-wall electrical parts, and an ultraviolet stabiliser intended for outdoor enclosures and high-light-exposure components. The exact flame-retardant chemistry is not identified here; it should be confirmed through the current safety data sheet and the UL Yellow Card because halogenated and halogen-free FR packages alter density, tracking resistance, and regrind stability. For class-equivalent 15% glass-fibre-reinforced FR UV PBT compounds, density is commonly reported between 1.49 g/cm³ and 1.54 g/cm³ according to ISO 1183-1. Compared with unfilled PBT, the 15% glass fibre raises tensile modulus and heat deflection temperature but reduces tensile strain at break and notched impact toughness. Compared with 30% glass-fibre FR PBT grades, the 15% fibre loading generally produces lower flexural modulus, lower specific gravity, and reduced warpage risk in flat connector housings. Table 1 provides class-typical property ranges based on published values for similar compounds and is not a lot-specific certificate.

    Because PBT undergoes ester hydrolysis in the melt in the presence of residual moisture, drying is the first process threshold. A desiccant dryer with a dew point of -30°C or lower should be used at 120°C for 3 h to 4 h; the target pellet moisture content is below 0.02% by weight, measured by ISO 15512 or Karl Fischer titration. In plants where relative humidity exceeds 60%, open pellet storage should be avoided because PBT can reabsorb moisture rapidly. If the compound is moulded with moisture above 0.03%, the resulting hydrolysis reduces molecular weight, lowers tensile elongation, and produces surface splay. Hot-air ovens are not an equivalent replacement for desiccant drying because their inability to reach low dew point can leave residual moisture above the safe limit even after extended heating. Production-scale failures reported in glass-filled PBT include gate-area delamination and reduced weld line strength after insufficient drying, particularly in thin-wall mouldings with wall thickness below 1.0 mm. The material must also be kept separate from polyacetal and PVC regrind; degradation products from those polymers are acidic and can accelerate PBT hydrolysis.

    What Limits the Injection Moulding Window for a GF15 FR UV PBT?

    Melt temperature measured at the nozzle should be maintained between 245°C and 260°C. The melt volume-flow rate for this class is commonly 10–25 cm³/10 min at 250°C and 2.16 kg according to ISO 1133-1:2022; the actual MVR for 3315GVU should be read from the lot certificate because it controls thin-wall fill pressure. Barrel settings from rear to front are commonly 240–250°C, 245–255°C, and 250–260°C, with the nozzle at 250–260°C. Temperatures above 270°C risk degrading the flame-retardant and UV additive package, which can shift colour and may compromise the UL 94 rating. At the opposite end, melt temperatures below 240°C produce high melt viscosity and can lead to short shots in sections thinner than 0.8 mm because PBT crystallises rapidly and solidifies at the flow front. Mould temperature should be held at 60°C to 80°C to promote crystallinity and stabilise dimensions; lower mould temperatures reduce surface gloss and can create post-mould shrinkage. On injection moulding machines with clamp force of 800–1,500 kN, the required hydraulic clamp force is generally 3–5 kN/cm² of projected area, similar to other glass-filled PBT grades. Total melt residence time should remain below 5–8 min; longer residence time increases MVR and can generate yellowing. If hot-runner systems are used, the hot-runner temperature should not exceed 250–260°C, and the residence time in the hot runner should be minimised to avoid pre-degradation. A general-purpose screw with L/D 20:1 and compression ratio 2:1 is usually adequate; high-shear screws with compression ratios above 3:1 can generate enough shear heating to exceed the 270°C limit even when barrel setpoints are lower. During screw recovery, back pressure between 0.3 MPa and 0.7 MPa is usually sufficient for homogenisation; higher back pressure can raise melt temperature by 5–10°C and shorten the thermal stability window.

    Glass fibre orientation dominates weld line strength and differential shrinkage. In glass-filled PBT, tensile strength measured on a double-gated ISO 527-2 specimen is generally lower than on a single-gated specimen, with weld line retention commonly between 45% and 60% for 15% glass fibre. The reduction in a 30% glass-filled PBT can be 30–45%, making the 15% grade preferable for parts with multiple gates or holes. Gate position should be placed away from structural ribs and snap-fit roots where possible. For film gates or large edge gates, land length between 0.5 mm and 1.0 mm is typical; the exact gate size should be adjusted to the part volume and flow length to avoid jetting. A double-gated ISO 527-2 specimen comparison should be used during tool qualification to quantify weld line loss, because part geometry and pigment can move the retention value.

    Dimensional Stability, Weld Lines, and Comparative Property Offsets

    For flat electrical housings, the 15% fibre loading provides an intermediate balance: less anisotropic shrinkage and warpage than 30% glass-filled PBT, but higher stiffness and heat resistance than unfilled PBT. Mould shrinkage for glass-filled PBT is anisotropic; class-typical total mould shrinkage is approximately 0.2–0.6% in the flow direction and 0.5–1.0% transverse to flow when measured on ISO 294-4 plaques. The exact shrinkage for 3315GVU depends on wall thickness, gate geometry, and pigment. Published multi-point shrinkage data for this specific configuration is limited; tool design should rely on boundary-flow simulation followed by a pilot tool trial. Dimensional stability after moulding is improved by the 15% reinforcement because the fibre reduces the linear coefficient of thermal expansion from approximately 8–12 × 10⁻⁵ K⁻¹ for unfilled PBT to about 3–5 × 10⁻⁵ K⁻¹ in the flow direction for a 15% fibre-filled PBT class, depending on orientation.

    Table 1 compares class-typical values for unfilled PBT, 15% glass-filled FR UV PBT, and 30% glass-filled FR PBT. The values are not lot-specific and are provided only as material-selection boundaries.

    PropertyTest methodUnfilled PBTKEPEX 3315GVU class-typicalPBT GF30 FR class-typical
    DensityISO 1183-11.29–1.31 g/cm³1.49–1.54 g/cm³1.55–1.65 g/cm³
    Tensile stress at breakISO 527-2 / ASTM D638-1450–65 MPa75–105 MPa100–135 MPa
    Tensile strain at breakISO 527-2100–200%2.0–4.0%1.5–3.0%
    Flexural modulusISO 178 / ASTM D790-172,400–2,800 MPa4,800–6,500 MPa7,500–10,000 MPa
    Charpy notched impact, 23°CISO 179-1/1eA4–8 kJ/m²3.5–6.0 kJ/m²5–8 kJ/m²
    HDT/A, 1.8 MPaISO 75-1/-2 / ASTM D648-1650–65°C185–205°C195–210°C

    The notched impact penalty of glass fibre is relevant in snap-fit designs. Unfilled PBT can yield at the base of a snap beam; the 15% glass-reinforced grade exhibits lower tensile strain at break, so snap-fit deflection should be limited below 2–4% outer-fibre strain. If the design requires high impact toughness, an unfilled PBT or a toughened PBT grade should be evaluated together with flammability requirements.

    Outdoor enclosure validation requires accelerated weathering and wet-service testing. The UV stabilisation package in 3315GVU is intended to reduce colour shift and surface chalking under solar exposure. For qualification, ISO 4892-2 xenon arc exposure or SAE J2527 automotive exterior weathering should be selected, and acceptance criteria should be expressed as ΔE, gloss retention, or the absence of surface microcracking after an agreed radiant energy interval. Published data for 3315GVU in long-term outdoor exposure are limited; colour-specific weathering reports from Korea Engineering Plastics should be required. In wet-service electrical applications, the combination of UV, humidity, and temperature can hydrolyse PBT; continuous exposure to hot water above 60°C is not recommended. If hot-water resistance is required, a hydrolysis-resistant PBT, PBT/PET blend, or PCT should be evaluated. Outdoor suitability claims under UL 746C should be confirmed by the described f1 rating and the UL file for the specific grade; published f1 status for 3315GVU is not stated here.

    Electrical connectors, relay bobbins, sensor housings, circuit-breaker internals, and outdoor telecommunication enclosures are typical application fields for this grade. The material should be evaluated against UL 94 at the minimum wall thickness in the final colour, because thin-wall flammability can change with pigmentation and glass content. Glow wire performance is commonly assessed by IEC 60695-2-12; the required glow wire ignition temperature depends on the end-product standard and may be 750°C, 850°C, or 960°C. Comparative tracking index should be tested according to IEC 60112; glass-filled FR PBT compounds commonly fall between 200 V and 250 V, but the exact value is compound-specific. Table 2 gives the compliance checklist that should be applied to the actual production lot.

    RequirementStandard/methodCommon condition or acceptance bandConfirmation step
    FlammabilityUL 94V-0 at 0.8 mm or 1.6 mm depending on colorUL Yellow Card for 3315GVU
    Glow wire resistanceIEC 60695-2-12GWFI 750–960°C, final wall thicknessSupplier test report
    Tracking resistanceIEC 60112CTI 200–250 V; lot-specific valueThird-party certificate
    UV stabilityISO 4892-2 or SAE J2527ΔE or gloss retention limit agreed by part specificationColor-specific weathering report
    Moisture after dryingISO 15512 / Karl Fischer<0.02% by weightIn-house moisture analyser
    Restricted substancesRoHS Directive 2011/65/EU, REACH Regulation (EC) No 1907/2006Product-specific declarationsSDS and supplier declaration

    When Should 3315GVU Replace PBT GF30 FR or a Non-UV PBT GF15?

    Selection of 3315GVU over a 30% glass-filled FR PBT is appropriate when warpage in flat parts is a primary defect or when lower part mass is desired. The 15% fibre loading reduces density and flexural modulus while retaining most of the heat deflection temperature of the 30% class. Selection over a non-UV FR PBT grade is indicated when the part is exposed to direct sunlight or high-level artificial light and colour stability is part of the acceptance specification. Selection over unfilled PBT is indicated when the part requires higher heat deflection temperature, lower thermal expansion, or greater dimensional reproducibility in thin-wall electrical connectors, provided that reduced ductility is accepted. If the application involves continuous flexural load at high strain or repeated snap-fit assembly, the lower tensile elongation of glass-reinforced PBT must be reviewed against ISO 527-2 stress-strain data. The material should not replace polyamide or polycarbonate without a review of dielectric properties, CTI, and moisture absorption because PBT offers lower moisture absorption but lower notched impact than many polycarbonate systems.

    Regrind use is permitted only after production validation. Repeated heat histories consume the UV stabilizer and can reduce UL 94 performance; the regrind fraction should be limited by test results for tensile strength, Charpy notched impact, and UL 94 at the minimum wall thickness. If regrind above 20–30% by weight is unavoidable, the moulder should verify that the mechanical property reduction remains within the part specification and that no surface defects appear at the gate after 50 consecutive shots. Production data for 3315GVU with high regrind ratios are limited; lot-specific validation is required.

    Top