| HS Code | 413767 |
| Grade | KEPEX PBT+GF15%-FR 3315GVS |
| Polymer Type | Polybutylene terephthalate (PBT) |
| Glass Fiber Content | 15% |
| Flame Retardant | Yes |
| Ul 94 Flammability Rating | V-0 |
| Density | 1.53 g/cm3 |
| Tensile Strength | 85 MPa |
| Tensile Elongation At Break | 2.5% |
| Flexural Modulus | 5500 MPa |
| Flexural Strength | 125 MPa |
| Notched Izod Impact Strength | 6 kJ/m2 |
| Heat Deflection Temperature At 1 8 Mpa | 190 °C |
| Heat Deflection Temperature At 0 45 Mpa | 205 °C |
| Melting Point | 225 °C |
| Mold Shrinkage | 0.4-0.8% |
| Water Absorption | 0.03% |
| Volume Resistivity | >1E16 ohm·cm |
| Dielectric Strength | 20 kV/mm |
| Processing Method | Injection molding |
As an accredited Korea Engineering Plastics KEPEX® PBT+GF15%-FR 3315GVS factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | KEPEX® PBT+GF15%-FR 3315GVS is supplied in 25 kg moisture-proof bags, 40 bags per pallet (1,000 kg), labeled and stretch-wrapped. |
| Container Loading (20′ FCL) | KEPEX® PBT+GF15%-FR 3315GVS is loaded in a 20-foot FCL container, packed in standard moisture-proof bags on pallets for safe shipment. |
| Shipping | KEPEX® PBT+GF15%-FR 3315GVS is shipped as non-hazardous plastic pellets in sealed moisture-barrier bags, typically 25 kg, palletized and stretch-wrapped. Transport and store in a dry, ventilated area under cool conditions, away from direct sunlight, heat, moisture, and contamination. Not regulated as dangerous goods for transport by road, sea, or air. |
| Storage | Store KEPEX® PBT+GF15%-FR 3315GVS in a cool, dry, well-ventilated area, away from direct sunlight, heat, ignition sources, and moisture. Keep in original, tightly sealed packaging and avoid static buildup. Separate from strong oxidizing agents. Protect from physical damage and prolonged high temperatures. Follow the manufacturer’s SDS and local regulations for safe handling and storage. |
| Shelf Life | Shelf life: typically 24 months when stored in original unopened packaging in a dry, cool, well-ventilated area. |
Competitive Korea Engineering Plastics KEPEX® PBT+GF15%-FR 3315GVS prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Korea Engineering Plastics KEPEX® PBT+GF15%-FR 3315GVS is a flame-retardant polybutylene terephthalate compound reinforced with 15% glass fiber by weight. The grade designation identifies a PBT matrix, 15% glass fiber loading, and a flame-retardant package configured for injection-molded electrical and electronic components. The compound is commonly supplied as cylindrical pellets of 3–4 mm nominal length. Certified values for density, tensile strength, flexural modulus, melt volume-flow rate, and flammability are those reported in the manufacturer’s technical data sheet and the UL Yellow Card; the following paragraphs use published comparative ranges for flame-retardant PBT compounds with 15% glass fiber loading rather than certified shipment values.
The glass fiber content of 15% positions the material between unfilled flame-retardant PBT and 30% glass fiber flame-retardant PBT. The formulation is intended for applications requiring UL 94 V-0 flammability classification, moderate stiffness, lower density than 30% glass fiber grades, and reduced moisture sensitivity compared with polyamide. Published data for this specific configuration is limited; therefore, application-specific testing under ASTM D638-14 or ISO 527-2 remains necessary for final part qualification.
Density of flame-retardant PBT with 15% glass fiber is typically 1.53–1.60 g/cm³ when measured by ISO 1183-1. The density differential against unfilled flame-retardant PBT is approximately 0.05–0.10 g/cm³, while a 30% glass fiber flame-retardant PBT is typically 1.65–1.75 g/cm³. The moderate glass content reduces anisotropic shrinkage relative to 30% glass fiber PBT and raises heat deflection temperature relative to the unfilled baseline.
Tensile strength at break measured by ISO 527-2/5 for comparable GF15 FR PBT grades usually lies between 85 MPa and 110 MPa, with elongation at break between 1.5% and 3.0%. Flexural modulus measured by ISO 178 is commonly 5,000–7,000 MPa; this is higher than unfilled flame-retardant PBT at 2,400–3,000 MPa but below GF30 flame-retardant PBT at 8,000–10,000 MPa. Notched Charpy impact strength at 23 °C by ISO 179-1/1eA is typically 3.5–6.0 kJ/m². Heat deflection temperature under 1.8 MPa by ISO 75-2/A is typically 195–210 °C. Melt volume-flow rate measured under ISO 1133-1:2022 at 250 °C and 2.16 kg is commonly 10–22 cm³/10 min for this class, which is lower than unfilled flame-retardant PBT because of the glass fiber content.
Because flame-retardant PBT compounds hydrolyze at melt temperatures above 260 °C, pre-drying is mandatory. The compound is dried in a desiccant dryer with a dew point below -30 °C at 120 °C for 4 h to reach a residual moisture content below 0.02%. Extended residence time above 4 min or melt temperature above 270 °C causes chain scission, volatile evolution, and discoloration. Hopper temperatures are maintained between 40 °C and 70 °C to avoid re-condensation of atmospheric moisture.
Injection molding uses a conventional three-zone screw with an L/D ratio of 18:1 to 22:1 and a wear-resistant non-return valve. Recommended melt temperature is 240–260 °C, mold temperature 60–90 °C, and back pressure 2–5 bar. Screw tangential speed is generally limited to 50–100 mm/s to minimize glass fiber breakage. Flow front velocity in thin-wall sections is held between 100 mm/s and 300 mm/s to avoid surface defects and excessive shear heating.
Barrel temperature profiles should be relatively flat, with a rear zone of 230–240 °C, middle zone of 245–255 °C, front zone of 250–260 °C, and nozzle at 250–260 °C. A temperature differential greater than 10 °C between adjacent zones can produce localized overheating and flame-retardant package degradation. Shot size should be controlled to 50–80% of barrel capacity; smaller shot sizes extend residence time, while larger shot sizes reduce plasticating uniformity. In production, batch-to-batch variation in flame-retardant dispersion can be observed if screw speed is too low or if the screw lacks dispersive mixing elements. Compounding of glass fiber into flame-retardant PBT is typically performed on a twin-screw extruder with an L/D ratio of 32:1 to 44:1, with glass introduced downstream by side feeding to preserve fiber aspect ratio.
Typical application areas include electrical connectors, relay bases, circuit-breaker housings, coil formers, lamp sockets, motor brush holders, sensor housings, and power distribution components. The grade is selected where the end product must satisfy UL 94 V-0 flammability classification at a certified thickness of 0.75 mm or 0.8 mm; the certified thickness for 3315GVS must be confirmed from the UL Yellow Card. Glow-wire ignitability testing is performed under IEC 60695-2-12, with flame-retardant PBT grades often assessed at 750 °C or 850 °C for unattended appliances. Comparative Tracking Index measured by IEC 60112 for brominated flame-retardant PBT grades is commonly 250–400 V; the 3315GVS value is grade-specific and appears on the UL Yellow Card.
Long-term thermal aging under UL 746B is required for exposed insulating materials. Typical flame-retardant PBT grades of this class exhibit a Relative Thermal Index electrical value near 130 °C and a mechanical impact value near 110–120 °C. Applications above these temperatures require external heat shielding or a higher-temperature polymer. Smoke density and corrosive gas emission may need to be assessed under IEC 60754-2 where railway or enclosed-building fire codes apply.
| Requirement | Standard / regulation | Typical status for GF15 FR PBT |
|---|---|---|
| Flammability | UL 94 V-0 at 0.75 mm or 0.8 mm | Certified thickness for 3315GVS from UL Yellow Card |
| Glow-wire ignitability | IEC 60695-2-12 | Assessed at 750 °C or 850 °C depending on end product |
| Comparative tracking index | IEC 60112 | Typical 250–400 V for brominated FR PBT |
| Restriction of hazardous substances | 2011/65/EU, (EU) 2015/863 | Supplier compliance statement required |
| REACH SVHC | EC 1907/2006 | Supplier confirmation required per lot |
Because polyamide 66 absorbs 2.5–3.0% moisture at 50% relative humidity, dimensions and electrical resistivity of PA66 GF15 flame-retardant grades shift during service. PBT-based 3315GVS moisture absorption under ISO 62 at 23 °C, 50% relative humidity is generally below 0.1%. This lower moisture uptake reduces post-mold dimensional growth and stabilizes comparative tracking performance in humid environments. The trade-off is a lower notched impact strength than polyamide and a narrower processing window, so polyamide may be preferred in load-bearing snap-fits subject to high strain rates.
For electrical connectors in tropical or condensing operating conditions, the selection of PBT over PA66 is often driven by the need to maintain creep resistance and dielectric strength after moisture conditioning. Comparative creep testing under ISO 899-1 at 80 °C shows PBT GF15 FR retains a higher percentage of initial flexural modulus than moisture-conditioned polyamide, though published data for 3315GVS specifically is limited. The lower equilibrium moisture content also reduces the risk of board-level corrosion around metal inserts in humid electronic enclosures.
The 15% glass fiber level is a design compromise. It increases tensile strength, flexural modulus, and heat deflection temperature relative to unfilled flame-retardant PBT, while retaining better flow and lower density than 30% glass fiber flame-retardant PBT. The table below provides indicative comparative ranges from public polymer databases for flame-retardant PBT grades; certified 3315GVS values are batch-specific.
| Property | Test method | Unfilled FR PBT | PBT GF15 FR | PBT GF30 FR |
|---|---|---|---|---|
| Density | ISO 1183-1 | 1.45–1.50 g/cm³ | 1.53–1.60 g/cm³ | 1.65–1.75 g/cm³ |
| Tensile strength | ISO 527-2/5 | 50–70 MPa | 85–110 MPa | 110–140 MPa |
| Flexural modulus | ISO 178 | 2,400–3,000 MPa | 5,000–7,000 MPa | 8,000–10,000 MPa |
| Notched Charpy impact, 23 °C | ISO 179-1/1eA | 3–5 kJ/m² | 3.5–6.0 kJ/m² | 7–10 kJ/m² |
| HDT/A 1.8 MPa | ISO 75-2/A | 120–150 °C | 195–210 °C | 200–220 °C |
| Mold shrinkage flow direction | ISO 294-4 | 1.2–1.8% | 0.4–0.8% | 0.2–0.6% |
Mold design for 3315GVS must account for glass fiber orientation. Gate dimensions should be at least 60% of the nominal wall thickness to avoid jetting and excessive shear heating. Full-round runner diameters of 4–6 mm are used for multi-cavity tools, with cold slug wells at each runner branch. Differential shrinkage between flow and transverse directions is lower than in 30% glass fiber flame-retardant PBT, but weld lines in complex connector housings still reduce local strength by 30–50% relative to the bulk material. Weld-line placement should be moved away from snap-fit corners and screw bosses by adjusting gate position or using sequential valve gating.
Glass fiber orientation also affects surface appearance. At 15% loading, mold surface replication is better than GF30 FR PBT but glass fiber readout can occur in thin polished areas. A mold temperature at the upper end of the 60–90 °C range, conservative packing pressure, and a textured cavity surface reduce visual defects. For high-gloss connectors, chemical foaming or post-plating is generally not recommended because flame-retardant PBT grades with glass fiber show limited metal adhesion.
Clamp force requirement is calculated from projected area and cavity pressure, which in thin-wall PBT parts typically reaches 300–500 bar. For a multi-cavity connector tool with a projected area of 250 cm², a press capable of 750–1,250 kN is usually selected. Undersized clamp force can produce flash at the parting line, while excessive clamp force distorts thin cores and vents poorly.
3315GVS is not suitable for continuous contact with strong acids, strong bases, or boiling water. Polybutylene terephthalate undergoes ester hydrolysis in hot aqueous environments above 80 °C, and the flame-retardant package can migrate at elevated temperature. Avoid combination with amine-based additives or some silicone-containing lubricants that can destabilize the flame-retardant synergist and reduce UL 94 V-0 performance. The material is also unsuitable for direct exposure to ketone-based solvents; short wipe resistance testing should follow ISO 22088-3 or ASTM D543 for specific chemical resistance data.
Post-consumer recycled content is not recommended for this grade unless a controlled closed-loop stream is available. Regrind from 3315GVS sprues and runners may be added at up to 20% by weight provided it has been dried and is free of contamination; higher regrind fractions increase the risk of black specs, glass fiber attrition, and inconsistent flame-retardant performance. Before regrind use, the molded part must be re-evaluated under UL 94 and IEC 60695-2-12 because the flame-retardant package is sensitive to repeated thermal history.