| HS Code | 964395 |
| Grade | KHBT2130 NC121 |
| Base Polymer | Polybutylene terephthalate (PBT) |
| Glass Fiber Content | 30% |
| Color | Natural |
| Density | 1.53 g/cm³ |
| Molding Shrinkage | 0.2-0.5% |
| Water Absorption 24 H | 0.1% |
| Tensile Strength | 120 MPa |
| Elongation At Break | 3% |
| Flexural Strength | 180 MPa |
| Flexural Modulus | 8500 MPa |
| Notched Izod Impact Strength 23 C | 9 kJ/m² |
| Hdt At 1 82 Mpa | 200°C |
| Melting Point | 225°C |
| Flammability Rating | UL94 HB |
| Dielectric Strength | 20 kV/mm |
| Volume Resistivity | 1E15 Ω·cm |
As an accredited Kanghui PBT+GF KHBT2130 NC121 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 25 kg moisture-barrier bags, stacked on pallets, each bag labeled with product code, batch number, and handling information. |
| Container Loading (20′ FCL) | Kanghui PBT+GF KHBT2130 NC121 is palletized in 25 kg bags, shrink-wrapped, and securely loaded into a 20′ FCL for export. |
| Shipping | Kanghui PBT+GF KHBT2130 NC121 is shipped as moisture-proof bags or octabins of glass-fiber-reinforced PBT pellets. Handle as a non-hazardous industrial thermoplastic unless the SDS states otherwise; keep dry, away from heat and sunlight, and avoid package damage. |
| Storage | Store Kanghui PBT+GF KHBT2130 NC121 in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat sources, flames, and moisture. Keep material in original sealed packaging on pallets; prevent bag damage, contamination, and deformation. Avoid prolonged exposure to high humidity or temperatures. Ensure FIFO stock rotation. Observe local regulations and the supplier’s SDS for safe handling and storage. |
| Shelf Life | Typically 24 months from date of manufacture when stored sealed in a cool, dry place, away from moisture and direct sunlight. |
Competitive Kanghui PBT+GF KHBT2130 NC121 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Kanghui PBT+GF KHBT2130 NC121 is a glass-fibre reinforced polybutylene terephthalate moulding compound supplied in a natural, unpigmented condition. The designation “NC121” identifies the natural-colour control; the exact glass-fibre mass fraction, melt-flow rate, and lot-specific mechanical values are confirmed by certificate of analysis rather than by the grade code alone. Under ISO 1043-1:2011 the material family is designated PBT-GF, and the ISO 11469:2016 marking code is >PBT-GF<. In comparison with unfilled PBT, the glass-fibre network raises tensile modulus, reduces mould shrinkage, and increases the temperature of deflection under load according to ISO 75-2:2013. The trade-off is a marked reduction in tensile strain at break and lower weld-line strength, which must be considered during gate placement and part design.
The natural, unpigmented form eliminates pigment-induced variation in thermal ageing and colour shift, but it does not contain carbon black to screen ultraviolet radiation. The grade is intended for opaque indoor service, painted parts, or applications in which UV exposure is minimal. Publicly available data for this specific configuration are limited; design work should use the manufacturer’s lot-specific data and production moulding trials rather than generic PBT+GF property tables. Natural-colour lot consistency is commonly assessed by CIE L*a*b* measurements under D65 illumination, with tolerances established in the incoming quality-control plan.
PBT is susceptible to hydrolytic chain scission if residual moisture is present during melting. The granules should be dried in a desiccant dryer at 110°C to 120°C for 3 h to 4 h, or until residual moisture is below 0.02 wt%. The dryer dew point should be maintained at or below -30°C. Hot-air hopper dryers alone are not sufficient when the processing environment exceeds 60% relative humidity, because PBT can re-absorb moisture during open hopper loading. In production, uncontrolled moisture appears as low melt viscosity, gate blush, silver streaks, and a measurable drop in tensile strength. A moisture analyser at the hopper throat is recommended for critical parts.
Injection-moulding barrel-temperature profiles are typically set with a rear zone of 240°C, a middle zone of 245°C to 250°C, a metering zone of 250°C to 260°C, and a nozzle at 250°C. Melt temperature should not exceed 270°C. Residence time in the barrel should remain below 5 min. During unscheduled stoppages, the screw should be purged with a stable PBT purge compound and the barrel temperature reduced to 160°C to 180°C. Prolonged residence above 270°C produces yellowing, viscosity loss, and surface deposits from ester-bond degradation.
Mould temperature is normally controlled between 60°C and 90°C. A surface temperature below 50°C can produce incomplete crystallinity and reduced chemical resistance. A mould temperature above 100°C improves crystallinity and weld-line appearance but increases cycle time. For thin-wall sections below 1.5 mm, high injection speed and holding-pressure profiling are used to prevent glass-rich surfaces and hesitation marks. Typical packing pressure ranges from 40 MPa to 80 MPa hydraulic, with holding time of 4 s to 10 s per 1 mm of nominal wall thickness.
On a reciprocating screw with 20:1 to 24:1 L/D and a compression ratio of 2.2:1 to 2.8:1, screw speed should generally be limited to 200 rpm to reduce glass-fibre attrition. Excessive screw speed reduces fibre length retention and tensile strength; insufficient screw speed increases recovery time and may cause melt stagnation in the compression zone.
Mould design must account for fibre-orientation-dependent anisotropic shrinkage. Shrinkage parallel to flow is typically lower than shrinkage transverse to flow. Ribs should be sized at 50% to 70% of the adjoining wall thickness to reduce sink marks. Gates should be placed at the thickest section, and any unavoidable weld line should be moved to a low-stress zone. In glass-reinforced PBT, weld-line tensile strength is commonly reduced to 50% to 60% of the base value because fibres do not bridge the weld interface.
For cavity-pressure sensing, a transducer located near the last fill point can confirm a packing pressure drop of 20 MPa to 35 MPa. This method is preferred over fixed timer-based packing because it compensates for viscosity shifts caused by lot-to-lot glass-fibre distribution and moisture variation. Production moulding is typically referenced to ISO 294-4:2018 test plaques for shrinkage verification.
The material is evaluated for mechanical design using ISO 527-2:2012 or ASTM D638-14 tensile tests on dry-as-moulded specimens conditioned at 23°C and 50% relative humidity. Glass reinforcement increases tensile modulus and tensile strength but reduces elongation at break. Notched Izod impact strength is measured according to ISO 180/A:2000; glass-filled PBT is more sensitive to gate and weld-line location than unfilled PBT. The table below summarises material-class screening ranges. These values are not lot-specific guarantees for KHBT2130 NC121 and must be replaced with certificate-of-analysis data for final design.
| Material / Property Method | Tensile Stress at Break (ISO 527-2 / ASTM D638) | Tensile Modulus (ISO 527-2) | Notched Izod (ISO 180/A) | HDT/A 1.8 MPa (ISO 75-2) | Mould Shrinkage (ISO 294-4) | Water Absorption 24 h (ISO 62) | CTI (IEC 60112) | UL 94 |
|---|---|---|---|---|---|---|---|---|
| Unfilled PBT | 50–60 MPa | 2.5–3.0 GPa | 3–4 kJ/m² | 50–60°C | 1.5–2.0% | 0.08–0.10% | 600 V | HB |
| Glass-fibre reinforced PBT, 15–20 wt% GF, natural | 90–110 MPa | 5.5–7.0 GPa | 5–7 kJ/m² | 195–205°C | 0.3–0.6% | 0.05–0.07% | 250–350 V | HB |
| Glass-fibre reinforced PBT, 30 wt% GF | 120–140 MPa | 9.0–11.0 GPa | 7–9 kJ/m² | 205–220°C | 0.2–0.5% | 0.04–0.06% | 200–300 V | HB |
| PA66+30 wt% GF, dry-as-moulded | 170–190 MPa | 9.5–11.0 GPa | 9–12 kJ/m² | 245–250°C | 0.3–0.5% | 0.7–1.0% at saturation | 500 V | HB/V-2 |
| Flame-retardant glass-filled PBT, V-0 at 1.5 mm | 100–120 MPa | 8.0–10.0 GPa | 5–7 kJ/m² | 190–205°C | 0.3–0.6% | 0.05–0.07% | 175–250 V | V-0 at 1.5 mm |
For electrical components, the comparative tracking index is measured according to IEC 60112:2003. Unfilled PBT can exhibit a CTI near 600 V, but glass reinforcement lowers the tracking resistance because surface erosion under electrical stress exposes glass-rich regions and accelerates carbon-path formation. In humid conditions, glass-filled PBT should not automatically inherit the CTI rating of an unfilled PBT grade. Volume resistivity and dielectric strength are determined by IEC 62631-3-1 or ASTM D257; end-product insulation coordination must follow the creepage and clearance requirements of IEC 60335-1 or IEC 60664-1.
Where dimensional stability in a humid environment is decisive, KHBT2130 NC121 is better suited than a dry PA66+30 wt% GF compound because the PBT backbone absorbs far less water. In switch housings, this reduces post-moulding warpage and contact-gap drift when relative humidity changes from 20% to 80%. However, low water absorption should not be confused with stable performance in hot water. Continuous immersion in water above 60°C can hydrolyse PBT ester bonds and cause surface cracking. For coolant-contact applications, PA66 or hydrolysis-resistant PBT grades should be selected.
Terminal blocks, relay sockets, connector housings, and coil formers are typical production applications for glass-filled PBT in electrical equipment because the material provides stiffness, low creep at ambient temperature, and adequate electrical insulation. In these applications, UL 94 HB may be acceptable for low-energy electrical enclosures, but the end-use product standard may require a minimum glow-wire ignition temperature or a V-0 classification. KHBT2130 NC121 should not be specified where V-0 at 1.5 mm is listed on the product safety drawing.
The substitution of a flame-retardant glass-filled PBT with KHBT2130 NC121 is not acceptable if the part certification depends on UL 94 V-0, glow-wire flammability index per IEC 60695-2-12, or a specific CTI class for printed-circuit-board connectors. The natural grade lacks the halogenated or phosphorus-based flame-retardant package required for V-0. If the application requires a living-part separation under IEC 60335-1, creepage and clearance must be re-evaluated because glass-filled PBT has a lower CTI than unfilled PBT.
Replacing a PA66+30% GF part with KHBT2130 NC121 is not a simple tensile-strength substitution. PA66 has a higher continuous service temperature and higher dry-specimen notched impact strength. In hot dry locations such as underhood air-intake housings, PA66 is generally preferred. In electrical housings exposed to high relative humidity, PBT+GF may be chosen because polyamide absorbs moisture, loses modulus, and changes dimension. A direct substitution should include comparative moisture ageing according to ISO 62:2008, tensile property retention after ageing, and constrained creep testing.
Compared with mineral-filled PBT, glass fibre gives higher tensile strength and greater fibre-orientation anisotropy. Compared with PBT/ASA or PBT/PC blends, the glass-reinforced grade offers higher ambient-temperature modulus but lower multi-axial impact at low temperature. A part designed for a ductile PBT/PC blend may crack under drop impact if converted to KHBT2130 NC121 without redesign. The product should therefore be treated as a stiff, creep-resistant PBT grade with limited ductility rather than a drop-in replacement for toughened blends.
Injection-moulding processing differences must also be observed when changing from flame-retardant PBT to a natural glass-filled PBT. Flame-retardant grades often require lower barrel temperatures to protect the flame-retardant package; KHBT2130 NC121 can be run with a standard PBT profile but must still be protected from moisture. A melt viscosity comparison should be made using ISO 1133-1:2022 at 250°C under 2.16 kg. If moulding is transferred from a high-flow unfilled PBT, higher injection pressure and larger gates may be required because glass fibres reduce melt flow and increase viscosity.
Avoid contact with hot strong alkalis, hot steam, and amine-containing mould-release agents. Strong alkaline cleaners at elevated temperature cause surface dulling and stress cracking. Avoid using this grade in continuous hot-water service above 60°C unless hydrolysis-resistant characteristics are separately confirmed. For outdoor components, UV stabilisation or painting is required; the natural grade is not intended for long-term direct sunlight.
| RoHS Directive 2011/65/EU | Restricted substances in electrical and electronic equipment; supplier declaration required. |
| REACH Regulation (EC) No 1907/2006 | SVHC candidate-list confirmation required at lot or product level. |
| ISO 1043-1:2011 | Designation PBT-GF for glass-fibre reinforced polybutylene terephthalate. |
| ISO 11469:2016 | Marking code >PBT-GF< for recycling and part identification. |
| ASTM D638-14 | Tensile test method for rigid plastics. |
| ISO 527-2:2012 | Tensile test method for moulding and extrusion plastics. |
| ISO 75-2:2013 | Temperature of deflection under load at 1.8 MPa. |
| ISO 1133-1:2022 | Melt volume-flow rate determination at 250°C under 2.16 kg for PBT. |
| IEC 60112:2003 | Comparative tracking index; glass reinforcement reduces the value relative to unfilled PBT. |
| UL 94 | Flammability classification; natural glass-filled PBT is typically HB unless modified. |
For first production runs, shot weight, cushion position, cycle time, screw recovery time, and peak injection pressure should be recorded to establish a baseline for detecting batch-to-batch variation. If a significant shift in melt viscosity occurs at constant moisture, the lot should be checked for glass-fibre content by ISO 3451-1 ashing. Because the grade code does not disclose fibre loading, a supplier lot change without an updated certificate of analysis may lead to overpacking, warpage, short shots, or moulded-in stress.