| HS Code | 560657 |
| Productname | Entec HYBOOST® 232 Masterbatch, LLDPE |
| Brand | Entec |
| Producttype | Masterbatch |
| Carrierresin | LLDPE |
| Additivetype | Proprietary |
| Additiveloading | 10% |
| Form | Pellets |
| Color | White |
| Density | 0.92 g/cm³ |
| Meltflowrate | 2.0 g/10 min (190°C/2.16 kg) |
| Meltingpoint | 125°C |
| Moisturecontent | <0.1% |
| Bulkdensity | 0.55 g/cm³ |
| Pelletsize | 2-3 mm |
| Recommendedprocessingtemperature | 180-220°C |
| Recommendedletdownratio | 2-5% |
| Fdacompliance | Compliant |
As an accredited Entec HYBOOST® 232 Masterbatch, LLDPE factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Entec HYBOOST® 232 Masterbatch, LLDPE is packaged in 25 kg moisture-resistant bags, palletized, and shrink-wrapped for safe storage. |
| Container Loading (20′ FCL) | 20′ FCL container loading for Entec HYBOOST® 232 Masterbatch, LLDPE: palletized, shrink-wrapped, strapped, and secured for safe export shipment. |
| Shipping | Entec HYBOOST® 232 Masterbatch, LLDPE is shipped as a non-hazardous polymer masterbatch in moisture-barrier bags, boxes, or octabins on pallets. Transport at ambient temperature, keep dry, avoid direct sunlight, and protect from contamination. No special transport classification; follow local regulations and SDS guidance. |
| Storage | Store Entec HYBOOST® 232 Masterbatch, LLDPE in a cool, dry, well-ventilated area away from direct sunlight, heat, ignition sources, moisture, and strong oxidizers. Keep original containers or bags tightly closed, off the floor, and away from food, feed, and drinking water. Avoid excessive stacking, dust, and static discharge. Use within recommended shelf life; rotate stock and follow local regulations. |
| Shelf Life | Entec HYBOOST® 232 Masterbatch, LLDPE has a 12-month shelf life when stored unopened in original packaging, cool, dry, away from sunlight. |
In single-layer and three-layer LLDPE blown film lines producing e-commerce mailers, void-fill sleeves, and protective wrapping, HYBOOST 232 is let down into the core layer or mixed with an LLDPE/LDPE dry blend at a starting-point screening range of 0.5 wt% to 2.0 wt%. On a three-layer line with a 250 mm spiral mandrel die, die gap 2.0–2.4 mm, and blow-up ratio from 2.2:1 to 2.8:1, gas evolution occurs mainly during the pressure drop at the die lip; one process conflict is that bubble stability falls when the frost line is raised above 600 mm from the die face because the reduced melt strength of the foamed core cannot withstand hoop stress variations. The LLDPE carrier in the masterbatch provides a melt viscosity closer to the base resin than a wax or EVA carrier would, but feed throat sticking is observed on lines with gravimetric hopper throat temperatures above 55°C; therefore throat cooling water is kept below 35°C. Where product-specific decomposition calorimetry for HYBOOST 232 is not available in the supplier data sheet, screw speed and barrel profile require confirmation by DSC or rheometric evaluation against analogous endothermic foaming masterbatches. For film testing, density reduction is measured according to ISO 1183-1:2019 and ASTM D1505-18; tensile and tear performance are benchmarked with ISO 527-3:2018 and ISO 6383-2. Outer layers are normally kept unfoamed at 5–10 µm each to preserve seal integrity, while the core layer may be reduced to 80–85% of its unfoamed density. Pre-drying at 60°C for 4 h is used only when storage relative humidity has exceeded 60%, because residual moisture creates pinholes and gel-like defects on the bubble surface.
Extrusion coating of paperboard and flexible substrates imposes a much shorter melt residence time than film blowing, and HYBOOST 232 is added to the LLDPE stream at 0.3 wt% to 1.0 wt% on a 90 mm single-screw extruder with L/D 30:1 and a barrier screw feeding a T-die with 0.8 mm lip opening. Melt temperature at the die is maintained between 205°C and 240°C; higher temperature accelerates gas evolution and causes foaming before the die exit, which appears as surface roughness and micro-pinholes in coatings below 15 g/m². The density drop from the foaming action lowers the required coat weight for a given barrier or cushioning task, but only if the melt strength of the LLDPE is adequate; low melt strength grades exhibit neck-in exceeding 50 mm at line speeds above 150 m/min. The pressure drop across the die lip nucleates cells that must not collapse before the chill roll freezes the surface; chill roll temperature is normally held at 15–25°C for gloss and adhesion. Adhesion is measured by cross-cut tape testing according to ISO 2409, while heat-seal strength of the coated substrate is verified according to ASTM F88/F88M-21. Because LLDPE is nonpolar, adhesion promoters or corona treatment above 40 mN/m may be required; the foaming masterbatch does not introduce polar groups that alter surface energy.
Thin-walled LLDPE packaging and industrial liners are injection molded with HYBOOST 232 added at 0.5 wt% to 1.5 wt% to reduce injection pressure requirement and minimize sink marks at bosses and ribs. On a hydraulic machine with clamp force from 1,000 kN to 2,500 kN, a general-purpose polyolefin screw with L/D 20:1 and compression ratio 2.5:1 is used; back pressure is kept at 0.5–1.0 MPa to disperse the masterbatch without pre-decomposing the blowing agent. Melt temperature is set between 190°C and 215°C, injection velocity between 80 mm/s and 120 mm/s, and hold pressure at 30–50% of injection pressure. Gas generated during filling lowers apparent viscosity and extends flow length, but vent depth on polyolefin tools must be maintained at 0.02–0.03 mm; shallower vents produce burn marks and gas traps at fill ends. Shrinkage is evaluated with ISO 294-4, tensile properties by ISO 527-2:2012 or ASTM D638-14, and notched impact by ISO 179-1. Sink mark depth is reduced mainly in sections where part thickness exceeds 2.5 mm; in very thin sections below 1.0 mm, cell collapse may occur rather than useful density reduction. Pre-drying at 60°C for 4 h is applied when the resin has been stored above 60% RH.
Extruded LLDPE sheet for thermoformed trays, dunnage, and reusable packaging is foamed with HYBOOST 232 at addition rates from 1.0 wt% to 2.0 wt% before a melt pump. A 120 mm single-screw extruder with L/D 32:1 and a barrier screw delivers melt at 180–210°C through a screen pack and gear pump into a 1,200 mm flexible-lip sheet die. The gear pump inlet pressure is held above 5 MPa to suppress premature foaming; if the pressure drops below 4 MPa, the dissolved gas expands before the die lip and creates prefoam melt fracture. After the die, the sheet enters a vertical three-roll stack at roll gaps from 2.0 mm to 4.0 mm; roll temperatures control skin thickness and surface smoothness. Apparent density is measured by ISO 845, tensile modulus and yield stress by ISO 527-2:2012, and flexural modulus by ISO 178. Foamed sheet exhibits lower flexural stiffness than solid sheet at equal thickness; therefore, load-bearing areas require ribbing or a thicker gauge. Published data for the exact density reduction achieved with HYBOOST 232 in this specific configuration is limited; screening trials are therefore run against a solid sheet control at the same thickness and same downstream draw ratio.
Rotational molding of LLDPE parts such as flotation aids, insulated containers, and double-wall tanks can use HYBOOST 232 when the masterbatch is pulverized with LLDPE powder to a particle size below 500 µm before charging. Addition rates are normally screened from 0.5 wt% to 1.5 wt% of the total dry-blend mass. The process imposes a conflict: oven temperature must be high enough to fully fuse the LLDPE powder, typically 250–300°C, but excessive mold temperature triggers gas evolution before the powder has densified, producing internal voids and rough inner walls. Peak internal air temperature for LLDPE is usually maintained between 180°C and 200°C; exceeding this range increases gas loss and pinholing. Gas evolution is therefore delayed by controlling mold heating time and by using a mold release that does not collect on the foaming surface. Rotational speed ratio is determined by tool geometry; for simple cylindrical parts a ratio of 4:1 is a common starting point, while asymmetric parts require independent calibration. Density is determined by ISO 845, tensile properties by ISO 527-2:2012, and impact energy by ISO 179-1. Published data for this specific configuration with HYBOOST 232 is limited; each tool geometry requires prototype runs because air cooling rate and mold wall thickness change cell structure more than in flat-sheet processes.
Foamed LLDPE insulation for twisted-pair and coaxial cable can be produced with HYBOOST 232 at let-down ratios from 0.3 wt% to 1.0 wt% in the insulation compound. The masterbatch is metered at the feed throat of a 60 mm single-screw extruder with L/D 30:1, feeding a crosshead die and pressure-cooling trough. Melt temperature at the die is held between 200°C and 230°C; gas evolution at the crosshead exit expands the insulation layer while the conductor speed is increased to maintain the required void fraction. Void fraction is verified indirectly by capacitance monitoring using IEC 61156-1 and directly by density measurement with ISO 1183-1:2019. Dielectric properties are tested according to ASTM D150-22. A smaller and more uniform cell size lowers the effective dielectric constant, but if cell size exceeds 50 µm or cell distribution becomes non-concentric, capacitance variance and return loss degrade. The LLDPE carrier in HYBOOST 232 avoids the viscosity mismatch that would occur with a polypropylene carrier in an all-LLDPE insulation compound.
Competitive Entec HYBOOST® 232 Masterbatch, LLDPE prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Entec HYBOOST® 232 Masterbatch is an LLDPE-carrier chemical foaming agent concentrate supplied in pellet form for polyolefin foam extrusion and structural foam injection moulding. The numerical designation 232 is a supplier grade code; it does not correspond to a generic additive loading. The linear low-density polyethylene carrier is a deliberate engineering selection: it softens within the processing window of polyethylene and, under controlled conditions, polypropylene, allowing the active foaming chemistry to be distributed into the melt without the dust burden of neat blowing agent powders. The product is intended for let-down dosing, not for use as a neat resin. Because the decomposition behaviour of the active system is thermally activated, the masterbatch must be processed within a bounded temperature and pressure window. Published data for this specific configuration is limited; where grade-specific values are not available, the statements below are derived from the documented behaviour of endothermic chemical foaming agents in LLDPE carriers.
The LLDPE carrier in HYBOOST® 232 lowers the melting point of the masterbatch relative to a high-density polyethylene carrier and creates a viscosity overlap with common extrusion and injection moulding grades. In polyolefin masterbatch practice, the carrier melt mass-flow rate is normally selected so that the masterbatch melt flow is greater than the base resin melt flow; this promotes shear-induced dispersion during the first melting stages. For base resins with an ISO 1133-1 melt mass-flow rate of 2 g/10 min to 20 g/10 min, the LLDPE carrier can be distributed by a single-screw extruder with a 24:1 to 33:1 length-to-diameter ratio. The carrier does not form a separate incompatible phase in polyethylene; in polypropylene, the LLDPE carrier exists as a minor discrete phase, and higher addition levels may reduce peak crystallinity and heat deflection temperature. Compatibility cannot be inferred from the carrier alone; the active foaming chemistry must also be dispersed below the decomposition onset to prevent prefoaming. The grade’s melt stability under shear is process-related: the use of high-shear mixing elements is acceptable only after a melt seal has formed, because upstream shearing of the solid masterbatch can generate frictional heat and initiate gas release in the feed zone.
For high-viscosity base resins outside the 2 g/10 min to 20 g/10 min window, the masterbatch may remain as visible inclusions if mixing is insufficient. In such cases, a Maddock or barrier mixing section is preferred over a pin mixer. The LLDPE carrier also contributes to feeding stability; pellet geometry and bulk density measured according to ISO 60 should be recorded because feeder calibration is affected by pellet-to-pellet size distribution. Published data for this specific configuration is limited.
The active chemistry in HYBOOST® 232 is classed as endothermic. During decomposition it absorbs heat and releases carbon dioxide and water vapour; the gas phase is therefore different from that of exothermic azodicarbonamide systems, which produce nitrogen, carbon monoxide, carbon dioxide, and ammonia-related species. Because the endothermic process draws heat from the surrounding melt, the temperature peak in the screw can be locally suppressed, and the melt viscosity may rise if too much gas is released before homogenization. Processing should start with the rear barrel zone below 160 °C to keep the LLDPE carrier from melting prematurely and to prevent gas liberation during solids conveying. Downstream barrel and die zones typically fall in the 200 °C to 230 °C range; the upper limit is bounded by residue stability and the onset of rapid degradation rather than by the carrier resin alone. The decomposition onset should be confirmed by differential scanning calorimetry according to ISO 11357-1/-2; a heating rate of 10 K/min under nitrogen is common for comparative tests. If the onset is below 160 °C, the screw temperature profile must be adjusted to delay gas release until a melt seal has formed.
Table 1 compares class-level behaviour of endothermic and exothermic chemical foaming masterbatches. The values are typical industrial ranges, not HYBOOST® 232 grade specifications.
| Parameter | Endothermic CFA masterbatch | Exothermic ADC masterbatch |
|---|---|---|
| Decomposition type | Heat absorbing; CO2 and H2O release | Heat releasing; N2, CO2, CO, NH3 release |
| Decomposition onset | 150 °C to 170 °C | 200 °C to 215 °C |
| Typical gas yield | 100 ml/g to 130 ml/g active chemistry | 200 ml/g to 220 ml/g active chemistry |
| Cell size trend | Fine cells, smoother surface | Coarser cells, higher foaming efficiency |
| Residue behaviour | Inorganic bicarbonate/citrate residue, lower plate-out | Organic residue, yellowness and plate-out risk |
The physical form of the masterbatch is pelletized, which improves metering accuracy and reduces fugitive dust compared with powdered blowing agent carriers. Pellets should be free-flowing; bulk density should be checked according to ISO 60 if gravimetric feeding systems are used. A batch-to-batch bulk density variation greater than 5 % can produce feed-rate drift on single-screw and modular volumetric dosing lines. Moisture is handled separately; the carrier itself is not highly hygroscopic, but the active chemistry may absorb surface moisture when bags are opened in high-humidity areas. Incoming moisture content greater than 0.15 % by ISO 15512:2019 Method A is a known source of surface blisters and gas-pressure fluctuation. Ash residue by ISO 3451-1 can be used as an incoming batch check for active loading; a deviation greater than the supplier’s acceptance band indicates a batch error that should be investigated before production.
In polyolefin foam extrusion, HYBOOST® 232 is dry-blended with the base resin and fed through the main hopper. Let-down ratios for endothermic CFA masterbatches in foaming are typically in the 0.5 wt% to 2.5 wt% range; the exact ratio for this grade must be established from the supplier’s datasheet and density-reduction trials. Below 0.5 wt%, cell nucleation may be insufficient to produce a uniform foam structure; above 2.5 wt%, carrier dilution of the base resin can lower melt strength and increase the risk of cell coalescence. The grade is suitable for sheet, profile, pipe, and cable sheathing lines where standard single-screw extruders are available. A barrier screw with a mixing head, screen changer, and melt pump is preferred because it maintains head pressure and reduces melt temperature fluctuation. The melt pump inlet pressure should be stable; pressure oscillations greater than ±5 bar are typically associated with feed surging or gas loss in the extruder.
Die design should account for the gas phase; for sheet and profile dies, the land length is often shorter than in solid extrusion because the gas expands at the die exit and an overlong land can induce prefoaming. A calibrator vacuum in the range of -20 kPa to -50 kPa is common for foamed profiles; the exact vacuum depends on the desired outer skin density. Extruder output may change with let-down ratio: on a 60 mm single-screw line with a 30:1 L/D screw, a shift of 0.5 wt% in masterbatch addition can change throughput because the gas phase reduces melt viscosity and shifts the die pressure characteristic. Published data for this specific configuration is limited.
In structural foam injection moulding, a shut-off nozzle is required to prevent drool and gas escape during screw recovery. Screw back pressure should be set high enough to homogenize the foamable melt but below the threshold that causes gas evolution in the metering zone. Typical hydraulic back pressure for foam moulding is 10 bar to 30 bar; plasticating speed should be adjusted to avoid high shear heating. Mould filling speed is critical: fill too slowly and gas escapes through the melt front before solidification; fill too quickly and gas bubbles can collapse or create weld-line defects. Short-shot trials should be performed with a gravimetric feeder and shut-off nozzle. The gate diameter for structural foam is often 1.5 to 2 times the solid-part gate diameter to reduce shear heating and premature gas separation. Gas counterpressure can be applied when the cavity is sealed and pressurised with inert gas at 10 bar to 30 bar before injection; this delays bubble expansion until the melt front reaches the end of the cavity and improves surface quality. Without gas counterpressure, expanding foam may leave swirl marks or blisters. Published data for this specific configuration is limited.
Density reduction is evaluated using ISO 1183-1 or ASTM D792-20; for structural foam parts, a reduction of 5 % to 20 % relative to solid parts is typical for endothermic systems, but the grade-specific maximum must be confirmed. Mechanical properties should be measured after conditioning at 23 °C and 50 % RH for 40 h according to ISO 291. Flexural modulus and strength should be measured according to ISO 178, and tensile properties according to ISO 527-2. For rigid polyolefin foam structures, cell size can be determined by ASTM D3576-20; for flexible foams, microscopy remains common because cell shape and orientation influence mechanical property interpretation.
Thermal blockage and melt sealing are central limits for HYBOOST® 232. If the feed-zone temperature is above 160 °C, the LLDPE carrier can soften too early and coat the screw root, reducing conveying efficiency. The resulting feed surging appears as pressure variation at the melt pump and changes the gas concentration entering the die. If the feed-zone temperature is below 140 °C, the polymer may not form a coherent melt plug before the active chemistry begins to decompose, allowing gas to vent backward toward the hopper. The practical feed-zone setpoint is therefore maintained at 140 °C to 160 °C, a 20 °C window that narrows when regrind content exceeds 30 wt% because regrind reduces bulk density and alters solids conveying. In a 30:1 L/D single-screw line, a feed-zone drift of 5 °C can move the melt-seal boundary forward by approximately one screw diameter; operators should record barrel setpoint and actual melt temperature to detect drift before it produces visible surface defects.
Melt pressure at the die is equally important. Carbon dioxide is soluble in polyolefin melts under pressure; if the melt pressure falls below the solubility limit at the local melt temperature, gas bubbles form in the die land and expand at the exit as frost lines, pits, or irregular cell distribution. Industrial practice on polyolefin foam lines often uses a head pressure alarm at 70 bar; below this value, prefoaming is likely in low-viscosity formulations. The necessary pressure depends on melt temperature, gas concentration, and base resin, so the alarm setpoint should be validated with the specific formulation. Increasing die resistance through a smaller die gap or a restrictive breaker plate can raise pressure without increasing melt temperature, but this also increases shear heating and may reduce output. If prefoaming appears as frost lines on the sheet or profile surface, the operating pressure should be increased by reducing die gap, increasing screw speed, or lowering melt temperature. A temperature reduction greater than 5 °C below the optimized profile may, however, move the decomposition reaction downstream and produce unreacted masterbatch. The practical melt-temperature control band is therefore often set to ±5 °C around the validated midpoint.
Moisture ingress affects HYBOOST® 232 even though the LLDPE carrier is hydrophobic. The active foaming system can absorb water from air when the package is open; the water is released as an additional volatile during processing and can create surface blisters, pinholes, and inconsistent cell structure. At relative humidity greater than 60 %, opened masterbatch should be pre-dried at 60 °C to 70 °C for 4 h in a dehumidifying dryer with a dew point below -30 °C. Drying above 80 °C should be avoided because the masterbatch may soften, agglomerate, or initiate premature decomposition of the active system. Moisture content before extrusion should be below 0.15 % by ISO 15512:2019 Method A. Closed, undamaged bags stored at 23 °C and 50 % RH in a dry warehouse generally require no drying, but bags should be reclosed immediately with a desiccant sachet after opening. If the material is exposed to condensation or high humidity for more than 8 h, drying is recommended. This moisture limit is a boundary condition; water vapour in the gas phase changes bubble nucleation and can produce open-cell structures in extrusion foams.
Shelf life for LLDPE-carried chemical foaming agent masterbatches is commonly 12 months in unopened original packaging stored at 23 °C and 50 % RH. Inventory should be rotated using first-in, first-out records. The product should not be stored near strong oxidising agents or open sources of heat; contamination with foreign polymeric pellets will alter the carrier-to-active ratio and should be rejected during incoming inspection.
Entec HYBOOST® 232 Masterbatch differs from exothermic ADC masterbatches in gas composition, residue behaviour, and decomposition heat. The endothermic decomposition releases carbon dioxide and water vapour, producing finer cells and lower plate-out in many polyolefin foaming applications. The trade-off is a lower gas yield per unit mass of active chemistry compared with ADC; therefore density reduction may require a higher addition rate. The use of an LLDPE carrier differentiates this grade from EVA-carrier and PS-carrier foaming masterbatches. LLDPE contributes to compatibility with polyethylene and avoids the low heat deflection temperature associated with EVA in many structural foam parts; in polypropylene formulations, the LLDPE carrier can be used but should be evaluated for effects on crystallization and stiffness. The product also differs from physical foaming systems using butane, pentane, or supercritical nitrogen and carbon dioxide: no separate gas injection pump, high-pressure saturation chamber, or modified screw is required, but the foaming gas is generated chemically and is coupled to the thermal and pressure conditions in the machine. For high-temperature polar polymers such as rigid PVC or polycarbonate, the LLDPE carrier and endothermic decomposition range are generally unsuitable; use of this masterbatch in such matrices can produce delamination and gas-escape surface defects.
Table 2 lists the compliance verification matrix applicable at the time of receiving inspection.
| Regulatory area | Document or standard | Verification point |
|---|---|---|
| REACH | Safety Data Sheet, Section 15 | SVHC status and exposure scenario |
| RoHS | 2011/65/EU with amendments | Pb, Cd, Hg, Cr(VI), PBB, PBDE |
| Food contact | FDA 21 CFR 177.1520 and EU 10/2011 | LLDPE carrier; active ingredients require end-use confirmation |
| Moisture | ISO 15512:2019 Method A | 0.15 % maximum before extrusion |
| Bulk density | ISO 60 | Incoming batch acceptance; maximum drift 5 % |
Bags should be stored flat, off the floor, and away from strong oxidising agents; inventory should be rotated using first-in, first-out records. The supplier’s Safety Data Sheet and technical datasheet should be consulted for batch-specific gas yield, ash residue, and maximum use level before production trials.