Ecoinvest Recycled Lldpe Granulate Colored Mfi 1 2 1 5

EcoInvest Recycled LLDPE Granulate Colored MFI 1.2-1.5

    • Product Name: EcoInvest Recycled LLDPE Granulate Colored MFI 1.2-1.5
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 194698
    Product Name EcoInvest Recycled LLDPE Granulate Colored MFI 1.2-1.5
    Material Recycled Linear Low-Density Polyethylene (LLDPE)
    Form Granulate
    Color Colored
    Melt Flow Index Mfi 1.2-1.5 g/10 min
    Density 0.920-0.940 g/cm³
    Melting Point 120-130 °C
    Tensile Strength 10-20 MPa
    Elongation At Break 400-800%
    Flexural Modulus 200-500 MPa
    Vicat Softening Temperature 90-110 °C
    Recycled Content 100%

    As an accredited EcoInvest Recycled LLDPE Granulate Colored MFI 1.2-1.5 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing EcoInvest Recycled LLDPE Granulate Colored MFI 1.2-1.5 is supplied in 25 kg moisture-resistant polypropylene bags, palletized and shrink-wrapped.
    Container Loading (20′ FCL) 20' FCL contains EcoInvest Recycled LLDPE Granulate Colored MFI 1.2–1.5 in 25 kg bags, palletized, shrink-wrapped, secured for ocean transport.
    Shipping EcoInvest Recycled LLDPE Granulate Colored MFI 1.2–1.5 is shipped as a non-hazardous solid polymer in 25 kg bags or bulk bags, palletized and stretch-wrapped. Transport in dry, covered trucks or containers at ambient temperature. Protect from moisture, contamination, and direct sunlight. Handle as normal industrial cargo; avoid sharp impacts and punctures.
    Storage Store EcoInvest Recycled LLDPE Granulate Colored MFI 1.2–1.5 in a cool, dry, well-ventilated area, away from direct sunlight, heat, flames, and strong oxidizers. Keep in original, closed bags or containers on pallets to prevent moisture, dust, and contamination. Avoid prolonged high temperatures, UV exposure, and static discharge. Maintain good housekeeping, rotate stock, follow local regulations, and protect from crushing.
    Shelf Life Shelf life is typically 12 months when stored cool, dry, sealed in original packaging, away from direct sunlight.
    Application of EcoInvest Recycled LLDPE Granulate Colored MFI 1.2-1.5

    In heavy-duty refuse sack and construction film extrusion, a recycled linear low-density polyethylene granulate with melt flow rate 1.2–1.5 g/10 min (ISO 1133-1:2022, Procedure A) is blended into film-grade LLDPE at 50–70 wt% to maintain bubble stability at blow-up ratios of 2.5:1–3.5:1. The pigment loading in the colored granulate restricts practical film thickness to approximately 60–200 µm; below that range, dart impact performance under ASTM D1709-16a becomes less consistent due to pigment dispersion limits. Compliance for finished sacks is assessed under EN 13592:2017, which governs household refuse sack dimensional and mechanical minima; tensile properties are tested according to ISO 527-3:2018, and tear resistance according to ISO 6383-1:2015. Recycled content claims are traceable under EN 15343:2007, with batch-to-batch melt flow rate deviation targeted at ±0.15 g/10 min. Extrusion is performed on a 55–75 mm grooved-feed single-screw blown-film line with an L/D ratio of 30:1, a die gap of 2.0–2.4 mm, and a dual-lip air ring; melt temperatures are held at 175–190 °C and die set temperatures at 175–185 °C. Surface moisture above 0.05 wt% measured by ISO 15512 Method A causes pinholes and should trigger pre-drying with dehumidified air at 65–75 °C for 2–4 h. Finished articles are limited to non-food contact heavy-duty refuse sacks of 70–120 L capacity, construction debris bags, scaffold sheeting, and temporary protective membranes. Use in food contact packaging under EU 10/2011 is not presumed and requires separate migration testing for the specific batch.

    How Does 15–30 wt% Recycled LLDPE Alter Parison Stability in HDPE Extrusion Blow Moulding?

    Addition of 15–30 wt% recycled LLDPE granulate into an HDPE blow moulding grade is used where environmental stress crack resistance and cold-temperature drop toughness are specified. The low MFI of 1.2–1.5 g/10 min provides higher melt strength than standard LLDPE injection grades and reduces uncontrolled parison sag in accumulator-head extrusion blow moulding machines with clamp force between 200 kN and 600 kN. Processing is carried out on an 80 mm screw diameter machine with 24:1 L/D, barrier screw geometry, melt temperature 195–210 °C, die head temperature 190–200 °C, and mould temperature 8–20 °C. The colored granulate should be pre-dried at 80 °C for 2 h when surface moisture exceeds 0.03 wt% by ISO 15512 Method A. Compliance for dangerous goods packaging is evaluated under UN Model Regulations Chapter 6.1 for plastics jerrycans and drums, including drop testing after conditioning at -18 °C; environmental stress crack resistance is measured by ASTM D1693-15 Condition B; heavy metal content is restricted by RoHS 2011/65/EU Annex II and REACH SVHC. Published comparative data for this specific colored compound is limited, so ESCR, drop impact, and melt flow ratio should be verified per lot before production. Typical terminal products are 20–30 L jerrycans, open-top industrial drums, automotive washer fluid reservoirs, and industrial lubricant containers. Addition above 30 wt% is not recommended in high-output lines exceeding 150 kg/h without melt fracture screening because surface roughness can increase.

    Thick-Walled Injection Moulding of Logistics Pallets, Crates, and Waste Containers

    Recycled LLDPE granulate at 10–25 wt% is let down into medium-flow HDPE injection moulding grades to raise notched Izod impact and low-temperature drop toughness in thick-walled logistics articles. The low MFI of 1.2–1.5 g/10 min limits flow length; therefore multiple hot runner gates spaced 200–300 mm apart are used on pallet moulds with nominal wall thickness 4–6 mm. Processing is executed on injection moulding machines with clamp force 10,000–25,000 kN, shot capacity 5–15 kg, screw L/D 20:1, compression ratio 2.5:1, melt temperature 210–235 °C, injection pressure 120–160 MPa, holding pressure 60–90 MPa, back pressure 0.5–1.5 MPa, and mould temperature 10–30 °C. Compliance for pallets is verified under ISO 8611-1:2011 for racking, stacking, and impact; dimensional stability under ISO 3394:2012; and material density under ISO 1183-1:2019. Recycled content claims follow EN 15343:2007. A grey or black colored granulate is preferred to prevent visible weld-line discoloration on large surfaces. Terminal products include 1200×1000 mm export pallets, collapsible distribution crates, agricultural harvest crates, and 120–240 L municipal waste container bodies. The upper addition limit is 25 wt% because above this level the pressure drop across hot runner systems rises and short-shot risk increases for flow length-to-wall-thickness ratios above 150:1.

    Compliance referenceParameterVerification scope
    ISO 8611-1:2011Racking, stacking, and impact1200×1000 mm export pallets
    ISO 3394:2012Plan dimensions and openingsDistribution crates
    EN 15343:2007Recycled content traceabilityAll batches
    ISO 1183-1:2019DensityAll batches

    Calendered containment membranes from recycled LLDPE with melt flow rate 1.2–1.5 g/10 min are processed on flat-die extrusion lines with 90–120 mm screw diameter, 30:1 L/D, die width 3,000–5,000 mm, and a three-roll polishing stack set to 65–85 °C. The formulation consists of 70 wt% recycled LLDPE granulate and 30 wt% virgin LLDPE to maintain stress crack resistance and sheet gauge uniformity between 0.75 mm and 2.00 mm. Melt temperature is held at 190–205 °C; melt pressure before the screen changer is limited to 200–280 bar to avoid gel formation from degraded colored fractions. Compliance references are GRI-GM17 for LLDPE smooth geomembrane properties, ASTM D5199-12 for nominal thickness, ISO 12236:2006 for static puncture resistance, and ASTM D5397-07 for notched constant tensile load stress crack resistance; recycled content traceability is under EN 15343:2007. This application is limited to temporary landfill covers, secondary containment liners, construction pit liners, and skip bin liners; it is not rated for primary containment of hazardous liquids or potable water contact without site-specific testing. At outdoor exposure, UV stabilizers must be compounded into the formulation at 1.5–2.5 wt% in the letdown because the base colored granulate alone does not guarantee 12-month weathering performance under ISO 4892-2:2013.

    When Recycled LLDPE Granulate Carries 20–40 wt% Calcium Carbonate in Twin-Screw Compounding

    Twin-screw compounding of filled polyolefin compounds uses the recycled LLDPE as the base resin because its MFI of 1.2–1.5 g/10 min permits high filler loading without torque overload on a 58 mm co-rotating twin-screw extruder with 40:1 L/D. The formulation comprises 60–80 wt% recycled LLDPE granulate, 20–40 wt% coated calcium carbonate with particle size 2–5 µm D50, and 1–3 wt% polyethylene-grafted maleic anhydride as compatibilizer. Compounding is run with side feeding at zone 6, melt temperature 190–215 °C, screw speed 450–650 rpm, and a gear pump before strand pelletization. Ash content is verified by ISO 3451-1:2019, filler dispersion by microscopy according to ISO 18553:2002, melt flow stability by ISO 1133-1:2022, and density by ISO 1183-1:2019. Such compounds are converted into industrial sheet, cable ducting, automotive wheel arch liners, and dunnage profiles. The operational boundary is 40 wt% filler; above that level, the compound melt flow rate may fall below downstream injection moulding requirements, and process-specific MFI verification per ISO 1133-1:2022 is required.

    Profile extrusion of edge protectors and industrial dunnage strips from recycled LLDPE granulate with melt flow rate 1.2–1.5 g/10 min is run on single-screw extruders with 45–60 mm screw diameter and 24:1 L/D, using a compact profile die and vacuum calibration tank. The formulation uses 80–100 wt% recycled LLDPE granulate and 0–20 wt% virgin LLDPE to adjust surface smoothness and haul-off consistency at line speeds of 6–15 m/min. Melt temperature is set at 180–200 °C; melt pressure before the breaker plate is limited to 150–220 bar. Compliance for weathering is verified under ISO 4892-2:2013 if outdoor use is specified; dimensional tolerance is checked according to ISO 3302-1:2014; recycled content traceability follows EN 15343:2007; and hazardous substance limits follow RoHS 2011/65/EU Annex II. The colored granulate produces opaque grey or black profiles with no post-extrusion painting. Terminal products include edge protectors for glass and sheet goods, industrial dunnage strips, racking buffer profiles, and conveyor guide rails. Pre-drying is required at 65–75 °C for 2–4 h if surface moisture exceeds 0.05 wt% by ISO 15512 Method A; above 1.0 wt% filler contamination from upstream recycling, screen packs of 80/120/80 mesh are recommended to prevent die lip buildup.

    Free Quote

    Competitive EcoInvest Recycled LLDPE Granulate Colored MFI 1.2-1.5 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    EcoInvest Recycled LLDPE Granulate Colored MFI 1.2-1.5, model designation EcoInvest LLDPE-R-C-1215, is a colored linear low-density polyethylene regranulate derived from sorted post-consumer and post-industrial film fractions. The melt flow index is specified as 1.2–1.5 g/10 min at 190 °C under 2.16 kg piston load in accordance with ISO 1133-1:2022 and ASTM D1238-20. Nominal density is 0.918–0.925 g/cm³ per ISO 1183-1:2019. The pellet geometry is cylindrical or lenticular, with average diameter 2.5–3.5 mm and length 3.0–4.5 mm; bulk density typically falls between 520 kg/m³ and 580 kg/m³. Moisture content at packaging is controlled below 0.10 % w/w by ISO 15512:2019. The product is supplied in carbon-black grey, mixed-color, and dark green families. Tight-color applications are outside the standard specification unless a separate pigment masterbatch is added because the CIE L*a*b* values vary with feedstock composition; customers requiring ΔE below 1.5 against a master standard must use an extruder-mounted dosing system.

    The material is not a direct drop-in replacement for prime LLDPE. Residual gel particles, non-polyolefin fragments, and colorant-related melt instability require adjustments to melt filtration, screw design, and film tower conditions. The low MFI range indicates a higher-viscosity film extrusion grade, but MFI alone does not capture the broader molecular weight distribution and oxidation history of recycled lots.

    What contaminant and gel limits separate recycled LLDPE from prime resins?

    Residual non-polyolefin contamination in post-consumer film is the principal technical boundary for this product. Paper fibre, polyester label fragments, ethylene-vinyl alcohol barrier scraps, aluminium foil laminates, and crosslinked gel particles from prior extrusion can pass into the regranulate if sorting and melt filtration are insufficient. Conversion lines should use a screen pack of 60/80/100 mesh or finer, and gear-pump-assisted melt delivery is recommended to stabilize pressure. Gel counts above 600 µm should be specified per application; in 50 µm blown film, acceptance criteria commonly require <150 gels/m² by camera-based gel inspection using a line-scan system. Lot-to-lot variation in gel count can shift film quality more than melt flow index variation, so a 2.0 mm die gap and increased head pressure are practical starting points on lines that normally run virgin LLDPE at 1.5 mm die gap.

    For single-screw extrusion, barrel profiles of 160/180/200/210/220 °C across five zones and melt temperature maintained at 200–230 °C are typical. The use of a barrier screw with L/D 24:1–30:1 and a Maddock mixing section reduces undispersed pigment agglomerates. Production-scale observations indicate that on a 75 mm extruder, screw speeds above 80 rpm can produce melt temperature overshoot above 230 °C when the recyclate contains oxidized film residues, increasing the rate of gel formation and reducing bubble stability downstream.

    Thermal degradation lowers OIT in colored recycled LLDPE

    Because the regranulate contains a mixture of original antioxidant packages, partial thermo-oxidative degradation products, and pigment-related metal ions, oxidative induction time is lower than that of a single virgin LLDPE film grade. The relevant test is ISO 11357-6:2018, run at 200 °C under oxygen. Lot-specific OIT must be verified before long-term heat-aging service; published data for this specific colored recyclate configuration is limited, and relying on generic recycled-polyolefin literature values is not recommended. Re-stabilization with hindered phenolic and phosphite systems at 0.1–0.3 wt% is commonly required when the granulate is used in agricultural film or geomembrane applications with expected service life above one year.

    At the feed throat, predrying is recommended when surface moisture exceeds 0.10 % w/w; drying at 65–75 °C for 2–4 h in a desiccant dryer with a dew point of -20 °C reduces steam bubble formation in thick-section profiles and stabilizes melt pressure in cast film. The material should not be blended with rigid PVC or PET regrind because melt-phase hydrolysis products from PET and chlorine from PVC can degrade the LLDPE chain and cause die lip corrosion on chrome-plated tooling.

    The low MFI range of 1.2–1.5 g/10 min places the product among higher-viscosity LLDPE film grades. In blown film, higher melt viscosity increases bubble stability, but also raises head pressure and melt fracture sensitivity. The apparent viscosity shift relative to virgin LLDPE depends on the molecular weight distribution and cannot be predicted solely from MFI; a capillary rheometer test per ISO 11443:2014 is therefore used for new color lots before line speed increases. At shear rates typical of film extrusion, the colored regranulate may require die temperatures 10–20 °C higher than natural virgin LLDPE to maintain the same output.

    When colored granulate replaces virgin LLDPE in blown film lines

    In blown film extrusion, die gap should be set to 1.5–2.0 mm, blow-up ratio held between 2.0:1 and 2.5:1, and frost-line height maintained at 8–12 die diameters to control bubble stability. The colored regranulate is more prone to sharkskin melt fracture at high shear stress because of the higher viscosity and inhomogeneous gel structure; reducing output by 10–20 % relative to virgin LLDPE under the same die diameter is a conservative starting condition. Melt pressure at the die entrance should be monitored rather than allowed to exceed 350 bar continuously; if pressure excursions exceed 20 % of the lot average, screen pack replacement or a lower screw speed should be used. Film produced from this grade is usually assigned to core layers, black or grey refuse sacks, industrial films, and temporary construction sheeting where minor gel defects and color variation do not impair function.

    Injection molding is limited to thick-wall parts. The melt flow index of 1.2–1.5 g/10 min produces high pressure drop in thin-wall sprues and runners, and wall thicknesses below 3 mm are generally outside the reliable processing window on clamp presses rated below 500 kN. Melt temperature should be 200–230 °C, back pressure limited to 50 bar, and injection speed set to the lowest setting that maintains complete filling to avoid shear heating and additional gel formation. Cushion and shot size should be adjusted for bulk density changes when switching from virgin pellets; the recycled pellets have a lower bulk density and may feed differently with a standard screw without a grooved barrel.

    The following table provides indicative property ranges for the granulate and reference polyolefin feedstocks. Values are supply-side ranges and are not lot-specific certificates of analysis.

    Comparative property ranges for recycled and virgin polyolefin film feedstocks
    PropertyTest methodEcoInvest LLDPE-R-C-1215Virgin LLDPE film gradeRecycled LDPE natural
    Melt flow indexISO 1133-1:20221.2–1.5 g/10 min0.8–2.0 g/10 min0.3–2.0 g/10 min
    DensityISO 1183-1:20190.918–0.925 g/cm³0.915–0.925 g/cm³0.915–0.935 g/cm³
    Tensile strength at yieldISO 527-2:201210–14 MPa12–20 MPa8–13 MPa
    Elongation at breakISO 527-2:2012500–800 %700–1000 %250–600 %
    Tensile modulusISO 527-2:2012150–250 MPa200–350 MPa100–200 MPa
    Moisture contentISO 15512:2019≤0.10 % w/w≤0.05 % w/w≤0.10 % w/w

    The principal difference between this grade and a virgin LLDPE is not the nominal melt flow index but the distribution of contaminants, colorants, and oxidized fractions. A virgin LLDPE film resin with MFI 1.0 g/10 min can be run at higher draw and thinner gauges, whereas the colored recyclate should be limited to gauges above 25 µm to avoid optical and gel defects. Compared with recycled LDPE, the LLDPE component in EcoInvest LLDPE-R-C-1215 provides greater puncture resistance and dart impact retention in film; however, the MFI band is narrower and lower than many recycled LDPE grades used in extrusion coating.

    Compliance matrix for recycled polyolefin shipments

    The following table lists regulatory boundaries that must be verified by the converter before specifying the product in a final article. Recycled content and food-contact status are not self-certifying across all lots.

    Regulatory and standard compliance matrix
    RequirementReference / methodEcoInvest LLDPE-R-C-1215 status
    REACH SVHC content 0.1 % w/wSupplier declaration under REACH Article 33Lot-dependent; pigment-specific verification required
    RoHS heavy metals: Pb, Hg, Cd, Cr6+2011/65/EU recastCarbon-black grey likely conforms; mixed colors require verification
    Food-contact polyolefinFDA 21 CFR 177.1520Not certified for direct food contact unless lot-specific documentation is issued
    Packaging heavy metal sum <100 ppmEU 94/62/ECColorant-dependent; mixed-color lots require testing
    Recycled content claimISO 14021:2016Supplier mass-balance audit available on request

    For multi-layer film structures, the granulate is typically processed as a core layer at addition rates of 20–40 wt% of the total film weight, with outer layers containing natural virgin LLDPE to maintain surface gloss and seal initiation temperature. Slot-die sheet extrusion at 200–220 °C is also possible for drainage boards, protective sheets, and packaging cores. In all cases, final article testing should include ash content, gel count, and OIT, because color and melt flow index alone do not capture the lot-to-lot variation introduced by the recycled feedstock.