Dupont Teijin Films Kaladex Pen Film Q83

DuPont Teijin Films Kaladex® PEN Film Q83

    • Product Name: DuPont Teijin Films Kaladex® PEN Film Q83
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 809470
    Density 1.36 g/cm³
    Melting Point 265 °C
    Glass Transition Temperature 121 °C
    Tensile Strength Md 200 MPa
    Tensile Strength Td 200 MPa
    Elongation At Break Md 100%
    Elongation At Break Td 100%
    Tensile Modulus Md 5500 MPa
    Tensile Modulus Td 5500 MPa
    Shrinkage 150c 30min Md 1.0%
    Shrinkage 150c 30min Td 0.5%
    Dielectric Constant 1khz 3.2
    Dissipation Factor 1khz 0.004
    Dielectric Strength 250 kV/mm
    Volume Resistivity 10^16 Ω·cm
    Water Absorption 0.3%
    Haze 1.5%
    Coefficient Of Friction 0.4

    As an accredited DuPont Teijin Films Kaladex® PEN Film Q83 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Supplied as 1 roll per carton, wound on a core and sealed in protective moisture-barrier packaging.
    Container Loading (20′ FCL) A 20-foot FCL container loaded with palletized DuPont Teijin Films Kaladex® PEN Film Q83, properly secured for ocean transport.
    Shipping DuPont Teijin Films Kaladex® PEN Film Q83 is shipped in protective rolls or sheets, securely packaged to prevent contamination, moisture, and mechanical damage. Store and transport in a clean, dry, ambient environment away from direct sunlight and heat; handle with care. Typically not regulated as dangerous goods.
    Storage Store Kaladex® PEN Film Q83 in a clean, dry, well-ventilated area, protected from direct sunlight, moisture, dust, and heat sources. Keep it in the original packaging, supported or rolled as supplied, and avoid prolonged exposure to high humidity or elevated temperatures. Keep away from solvents and contaminants, avoid heavy stacking, and follow first-in, first-out stock rotation.
    Shelf Life Q83 shelf life: typically 12 months from manufacture when stored unopened in original packaging at 15–25°C and 30–70% relative humidity.
    Free Quote

    Competitive DuPont Teijin Films Kaladex® PEN Film Q83 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    DuPont Teijin Films Kaladex® PEN Film Q83 is a biaxially oriented poly(ethylene 2,6-naphthalate) substrate produced from naphthalene-2,6-dicarboxylic acid and ethylene glycol. The Q83 designation appears in converter documentation for printed electronics, high-temperature labelling, flexible flat cable insulation, membrane touch-switch circuits, capacitor and battery insulation, RFID antenna substrates, and dimensionally stable laminates. Because the naphthalate ring replaces the terephthalate unit of conventional polyethylene terephthalate, the film exhibits a higher glass transition temperature, lower gas transmission at equal gauge, and better retention of mechanical properties after exposure to elevated temperature. Supplier-published Q83-specific data are less complete for certain optical and surface-energy values than for the broader Kaladex PEN platform; numerical values in this document therefore refer to representative Kaladex PEN film data unless a Q83-specific certification value is stated. Converters should validate all critical values against the current DuPont Teijin Films technical data sheet for the exact lot and gauge.

    The grade is evaluated primarily as a high-temperature polyester replacement for PET in flexible electronic and labelling applications. It is not a polyimide. Where process temperatures exceed 200 °C for sustained periods, polyimide remains the substrate of choice. The Q83 specification is therefore most relevant for converters that require a usable thermal plateau above PET but below the cost and colour limitations of polyimide.

    Thermal Stability, Shrinkage, and Dimensional Control from 20 °C to 200 °C

    Differential scanning calorimetry of Kaladex PEN film per ASTM D3418 records a glass transition near 120 °C and a crystalline melting endotherm near 269 °C. The corresponding PET glass transition is approximately 78 °C; the elevated transition is associated with reduced chain mobility at processing temperatures where PET begins to relax and distort. Unrestrained shrinkage measured at 150 °C for 30 min under ASTM D1204 is typically below 0.8 % in machine direction and below 0.5 % in transverse direction. At 200 °C the shrinkage increases rapidly, and web registration becomes sensitive to local thermal gradients. The coefficient of linear thermal expansion is commonly reported in the range 20–25 ppm/K for oriented film, which is lower than many amorphous PET grades and more compatible with copper-clad flexible-circuit processing. UL relative thermal index values for similar Kaladex PEN films are typically between 150 °C and 160 °C for electrical retention; Q83-specific RTI should be drawn from the supplier’s UL file.

    On stenter-frame production lines, the narrow dimensional window at 200 °C imposes a practical cross-web temperature uniformity of ±5 °C. Variations above this band produce registered die-cut error and curl in foil laminates. Published data for this specific Q83 configuration are limited; converter trials are used to establish the actual control band for a given line. The film clips and chain-track zones at the edges of the stenter can also create locally higher orientation stress. Converters frequently slit 10 mm to 20 mm from each edge before lamination or die-cutting to remove the edge region where thermal and mechanical history is least uniform.

    What Limits Moisture, Oxygen, and Solvent Transmission Across Thin-Gauge Q83?

    Barrier measurements on Kaladex PEN film follow standard flat-film methods. At 25 µm gauge, oxygen transmission measured at 23 °C and 0 % relative humidity under ASTM D3985 typically falls in the range 18–25 cm³/(m²·day·atm). Water vapour transmission measured at 38 °C and 90 % relative humidity under ASTM F1249 is typically 4–6 g/(m²·day) at the same gauge. These rates are approximately 50 % to 60 % lower than oriented PET at the same thickness. The reduction is not linear across all humidity conditions, and oxygen barrier improves at low relative humidity. The naphthalate structure also restricts the solubility and diffusion of aliphatic hydrocarbons and many aroma compounds; polar solvents, ketones, and chlorinated hydrocarbons can still attack the surface, especially at temperatures above 60 °C.

    Optical transmission for clear Kaladex PEN film is generally above 87 % with haze below 1.5 % under ASTM D1003. Where Q83 is used for backlit membrane switches or coverlay windows, the lower moisture uptake compared with PET preserves dimensional flatness in high-humidity assembly environments. The naphthalate chromophore also provides partial ultraviolet absorption in the 320–380 nm range, which can retard UV-induced embrittlement in outdoor-facing label stock. Long-term weathering under ISO 4892-2 shows better tensile retention than PET films of similar gauge, although Q83-specific weathering data are not uniformly published.

    For roll-to-roll coating and lamination, Q83 is typically processed in the biaxially oriented state. Predrying of the film is not required for standard adhesive lamination but may be required for extrusion coating where moisture in the coating resin, not the film, controls adhesion at line speeds above 50 m/min. Corona treatment of Q83 surfaces at 1.5–2.5 kW per metre of electrode width raises wetting tension to 48 mN/m or higher, and treatment decay is slower than PET because of limited migration of low-molecular-weight esters. On flat-bed die-cutting lines, registration drift across a 600 mm web has been observed when the film is not annealed; pre-annealing at 170 °C for 30 min under low tension reduces the drift to below 0.1 mm. Published data for the Q83 grade is limited, and converter trials should define the actual anneal cycle for a given laminate construction.

    Hard-coating and conductive-ink adhesion failures are commonly traced to inadequate surface oxidation rather than bulk resin defects. X-ray photoelectron spectroscopy of corona-treated PEN surfaces shows that silver-paste peel strength improves when the oxygen-to-carbon ratio rises above 0.25. On high-speed inkjet and rotary screen lines, the rewind tension for 25 µm film should be reduced relative to PET because the higher modulus changes bending radius and can produce telescoping or blocking at idler rolls. These are production-scale failure modes, not intrinsic property limits.

    When the naphthalate backbone displaces PET in high-temperature labels and printed circuits

    In high-temperature label stock and flexible printed circuits, Q83 is used where PET fails to survive downstream solder reflow, lamination, or autoclave exposure. The continuous-use window of 150 °C to 160 °C allows processing that would exceed the 105 °C to 120 °C mechanical ceiling of standard PET. Thermal shrinkage at 150 °C remains below 0.8 %, whereas PET may exceed 1.5 %. The film is also specified in RFID antenna substrates, flat-cable insulation, capacitor and battery insulation, and tactile switch spacers because it combines lower moisture absorption than polyimide with adequate electrical insulation. In comparison with polyimide, Q83 is not suitable for continuous service above 250 °C; however, its lower cost and higher optical clarity often justify selection in applications where peak temperature remains below 200 °C for short intervals.

    For flexible printed circuits, the dimensional stability of Q83 under adhesive lamination is a critical difference from PET. Copper-clad laminates made with PET can show curl and misregistration after the first high-temperature exposure; PEN-based laminates retain flatter geometry. Published data for this specific Q83 configuration are limited, but the platform property set is consistent with lower residual stress accumulation during foil lamination at 160 °C. Q83 should not be selected for solder float above 260 °C or for direct chip-on-flex bonding that requires polyimide-level thermal endurance.

    Dielectric Response and Surface Treatability after Corona Exposure

    At 25 µm gauge, dielectric strength measured under ASTM D149 is usually reported between 250 and 300 kV/mm. Dielectric constant at 1 kHz is approximately 3.0, and dissipation factor is below 0.005. Surface resistivity measured under ASTM D257 is typically 10^15 to 10^16 Ω/square at 23 °C and 50 % relative humidity. Q83-specific dielectric values should be confirmed for the exact gauge, because thinner films can show different apparent breakdown behaviour due to electrode geometry and defects.

    Representative physical-property window for the Kaladex PEN platform; Q83-specific certification values should be drawn from the current supplier technical data sheet.

    PropertyTypical value or rangeUnitTest method
    Density1.36g/cm³ASTM D1505
    Tensile strength at break250–275MPaASTM D882
    Elongation at break60–80%ASTM D882
    Young’s modulus5–6GPaASTM D882
    Glass transition120°CASTM D3418
    Continuous-use temperature150–160°CUL 746B platform data
    Oxygen transmission, 25 µm18–25cm³/(m²·day·atm)ASTM D3985
    Water vapour transmission, 25 µm4–6g/(m²·day)ASTM F1249
    Dielectric strength, 25 µm250–300kV/mmASTM D149
    Surface resistivity10^15–10^16Ω/squareASTM D257

    Chemical resistance is evaluated by immersion in 10 % sodium hydroxide and 10 % sulfuric acid for 48 h at 23 °C. The naphthalate structure shows lower hydrolysis sensitivity than PET, although strong alkaline solutions at elevated temperature still attack the ester linkage. Q83 is not resistant to all organic solvents; ketones and chlorinated hydrocarbons may haze or swell the film depending on concentration and exposure time. Regulatory declarations are typically available for RoHS Directive 2011/65/EU as amended by (EU) 2015/863, REACH Regulation (EC) No 1907/2006, and EU food-contact Regulation 10/2011 for certain clear and treated grades. Converters must obtain the Q83-specific declaration because surface treatment and additive package can alter the regulatory status.

    Comparative property windows for oriented PEN, PET, and polyimide films; values are typical industrial ranges and are not Q83-specific.

    PropertyKaladex PEN platformPET filmPolyimide film
    Glass transition120 °C78 °C350–400 °C
    Continuous-use temperature150–160 °C105–120 °C240–300 °C
    Moisture absorption0.4 %0.6 %2.5–2.9 %
    Oxygen transmission, 25 µm18–25 cm³/(m²·day·atm)50–60 cm³/(m²·day·atm)>100 cm³/(m²·day·atm)
    Thermal shrinkage at 150 °C<0.8 %>1.5 %<0.1 %
    Optical appearanceClear to slightly amberClearAmber

    Substituting Q83 into Existing PET Conversion Lines: Known Process Boundaries

    The substitution of Q83 into a line designed for PET is not a drop-in replacement. Tension settings that operate safely with 25 µm PET can induce curl in Q83 because the higher modulus changes the bending radius at dancer rolls and idlers. Drying requirements are different: although oriented film is dry to water, pre-annealing at 170 °C is often required to remove residual orientation stress before blanking or punching. The film also has a narrower thermal window at 200 °C; cross-web temperature variation above ±5 °C can produce transverse distortion. Alkaline cleaners at temperatures above 80 °C should be validated, because the ester linkage remains susceptible to hydrolysis under high-pH, high-temperature exposure. Q83 is not recommended for continuous service above its UL relative thermal index, for direct steam exposure above 120 °C without barrier lamination, or for applications requiring polyimide-grade performance at solder float temperatures above 260 °C.

    Hydrolysis kinetics in hot, saturated humidity are more favourable for PEN than for PET, but the margin is not unlimited. In retort conditions at 121 °C, PET laminates can lose a significant fraction of tensile strength within 24 h depending on pH; PEN retains a greater fraction for a longer interval. Published data for this specific Q83 configuration are limited, and converters should not extrapolate from generic PEN retort values without lot-specific testing. Adhesive systems containing high-residue acid catalysts or aggressive cleaning chemistries should also be evaluated for surface attack before full-scale qualification.

    Top