| HS Code | 506541 |
| Thickness | 50.8 µm |
| Density | 0.920 g/cm³ |
| Tensile Strength At Break Md | 24.8 MPa |
| Tensile Strength At Break Td | 22.1 MPa |
| Elongation At Break Md | 600% |
| Elongation At Break Td | 700% |
| Elmendorf Tear Strength Md | 200 g |
| Elmendorf Tear Strength Td | 400 g |
| Dart Drop Impact | 140 g |
| Haze | 10% |
| Gloss | 80% |
| Coefficient Of Friction | 0.2 |
| Heat Seal Initiation Temperature | 105°C |
| Water Vapor Transmission Rate | 15 g/m²/24h |
| Oxygen Transmission Rate | 2000 cc/m²/24h |
As an accredited DuPont™ Sclairfilm® GL-1 LLDPE Film, Laminating, 50.8 µm Thickness factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Each carton contains one 50.8 µm thick DuPont™ Sclairfilm® GL-1 LLDPE laminating film roll, wrapped in protective moisture-barrier packaging. |
| Container Loading (20′ FCL) | 20′ FCL: Palletized rolls of DuPont™ Sclairfilm® GL-1 LLDPE laminating film, 50.8 µm, loaded, secured, and moisture-protected for ocean shipment. |
| Shipping | DuPont™ Sclairfilm® GL-1 LLDPE Film, 50.8 µm, ships as non-hazardous plastic film on rolls, wrapped in protective moisture-barrier packaging, boxed and palletized. Store and transport dry at ambient temperature, away from sunlight, heat, moisture, and sharp objects. Handle cleanly; avoid excessive stacking. Follow manufacturer SDS and local regulations. |
| Storage | Store DuPont™ Sclairfilm® GL-1 LLDPE Film in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, flames, and moisture. Keep rolls in original packaging, sealed until use, to prevent dust, contamination, and physical damage. Protect from crushing, punctures, and sharp objects. Avoid prolonged UV exposure. Maintain moderate temperatures and follow supplier SDS and local regulations. |
| Shelf Life | Shelf life is 12 months from date of manufacture when stored in original packaging at temperatures below 30°C, away from direct sunlight and moisture. |
DuPont™ Sclairfilm® GL-1 as a 50.8 µm LLDPE laminating web is most frequently placed as the heat-seal side of a two-component dry-lamination structure for dry snack and confectionery packaging. A reverse-printed 12–20 µm BOPP or PET outer web is bonded to the LLDPE film with a solventless aliphatic polyurethane adhesive at a coat weight of 1.8–2.5 g/m²; the laminator nip temperature is held between 60 °C and 75 °C, and the reels are conditioned at 35 °C and 50 % RH for 48–72 h before slitting. The corona-treated side of Sclairfilm GL-1 is specified at 38–42 mN/m according to ASTM D2578; below this range, solventless adhesives can retract from the substrate, producing optical mottle and low laminate bond strength. In subsequent vertical form-fill-seal operations, jaw temperatures from 115 °C to 145 °C with 0.30–0.50 s dwell and 276–414 kPa seal pressure are typical converter settings for a 50.8 µm LLDPE sealant layer. Seal strength is normally verified to a minimum of 2.5 N/15 mm after 24 h using ASTM F88/F88M, and hot-tack values in the range 2.0–4.0 N/15 mm at 120 °C are accepted for products that drop onto the bottom seal before cooling. The principal processing conflict is the modulus difference between the oriented outer web and the LLDPE sealant: polyester may have a tensile modulus roughly 20–30 times that of LLDPE. When the secondary unwind tension is too low, the laminate forms transverse tunneling; when it is too high, the 50.8 µm web necks and the cured laminate curls toward the polyester face. Production laminators therefore run closed-loop load-cell unwind tension near 0.5–1.0 N/mm of web width for the sealant web while the primary web runs at 1.5–2.5 N/mm. Incoming film inspection for Sclairfilm GL-1 includes thickness profile per ASTM D374, tensile properties per ASTM D882, and heat-seal curve generation per ASTM F1921. A thickness variation greater than ±10 % across the web can produce alternating seal strengths at the fin-seal jaw because the seal bar pressure is not redistributed uniformly. Slitting with dull shear knives generates hazy edge defects and particulate contamination in the seal zone; converters therefore replace blades at intervals determined by the percentage of edge dust rather than by footage alone.
A reverse-printed PET or BOPP outer web laminated to 50.8 µm Sclairfilm GL-1 is used for frozen vegetable bags, seafood pouches, and IQF poultry packages because the sealant must survive rapid temperature drops from ambient filling to -20 °C or -40 °C without brittle fracture. The LLDPE layer is selected over low-density polyethylene at equal gauge because its low-temperature ductility reduces seal-area cracking when filled bags are sharply folded or dropped. Validation work on production freezers generally evaluates seal strength per ASTM F88/F88M at room temperature and again after 24 h at -18 °C; acceptable packages retain destructive seal separation rather than cohesive seal fracture at the package corners. Impact testing of the laminate is carried out using ASTM D1709 dart drop or ASTM F1306 puncture after low-temperature conditioning, although published data for this specific laminating grade under frozen conditions is limited and therefore must be generated for each structure. The same limitation applies to oxygen barrier: a plain 50.8 µm LLDPE web does not provide sufficient gas barrier for oxygen-sensitive frozen sauces or fish; the structure must include aluminum foil, metallized PET, or an EVOH-containing core. Thermal shock occurs when the filled pouch passes from ambient filling to blast-freeze tunnels at -35 °C; the sealant layer must track the shrinkage of the outer web without delaminating. If the PET or BOPP outer web shrinks more than the LLDPE layer, the laminate can show a negative curl and seal-area microcracks that are detected only after the package is flexed. Converter countermeasures include specifying a low-shrink outer web, maintaining adhesive coverage above 2.0 g/m², and slitting the laminate with sharp shear knives to avoid edge-initiated tears. The critical quality point is not the initial seal temperature but the seal-bar temperature uniformity across the fin-seal jaw. A drop of ±5 °C across the jaw can produce alternating weak zones and heavy weld zones, especially when the machine operates above 60 bags/min.
For medical device sterile barrier pouches, 50.8 µm Sclairfilm GL-1 can be used as the sealant web in film-to-film and film-to-Tyvek configurations. In a typical film-to-Tyvek pouch, the outer layer is a polyester/polyethylene laminate or a paper/plastic laminate, and the LLDPE sealant side is heat-sealed to uncoated Tyvek at 120–143 °C, 275–414 kPa, and 0.5–1.0 s dwell. Seal validation under ISO 11607-1 and ASTM F88/F88M is mandatory; many device manufacturers accept a minimum seal strength of 1.0 N/15 mm, but the validated limit must be derived from the specific pouch configuration and sterilization load. Coated Tyvek is generally preferred for peelable openings; Sclairfilm GL-1 is not a peel-fusion film, so the peel function must be supplied by a peelable coating or by controlled delamination of the substrate. Gamma irradiation at 25 kGy may shift the sealant’s elongation and seal strength; accelerated aging per ASTM F1980 is used to estimate real-time shelf life, but published data for this exact film after gamma exposure is limited. Ethylene oxide sterilization is less damaging to polyethylene sealants, but aeration must remove residual gas from the seal area, and the pouch must be validated for microbial barrier per ASTM F1608 if the structure is porous. The manufacturing constraint is seal-bar temperature distribution: on a 600 mm sealing bar, a ±5 °C variation can produce channel leaks at the chevron corners, so continuous temperature mapping and periodic destructive burst testing per ASTM F2054 are standard. The film complies with FDA 21 CFR 177.1520 for olefin polymers and with European Union food-contact legislation when supported by migration data; for medical use, biocompatibility of the finished device package remains the responsibility of the device manufacturer.
Liquid portion packs for edible oil, condiment, isotonic beverage concentrate, and low-viscosity detergent are frequently converted as PET/foil/LLDPE laminates in which the 50.8 µm Sclairfilm GL-1 web is the innermost sealant. The aluminum foil, usually 7–12 µm, provides the gas barrier; the LLDPE layer contributes flex-crack resistance and a broader seal-temperature tolerance than low-density polyethylene. Adhesive lamination with solvent-based or solventless polyurethane is run at 2.0–3.0 g/m² coat weight, with the higher end used when foil is present because foil’s thermal conductivity draws heat from the curing adhesive and can slow crosslinking. Gelbo flex testing per ASTM F392 after 50 or 100 cycles is used to quantify pinhole formation; LLDPE sealant layers of this thickness are more resistant to flex cracking than LDPE at the same gauge, but the absolute pinhole count also depends on the flexing mode and foil gauge. On horizontal liquid pouch machines, the bottom seal is made while product is already present or is dosed immediately after sealing, so the sealant must tolerate a moist, cold product environment. Seal bar settings of 120–150 °C, dwell 0.4–1.0 s, and pressure 276–483 kPa are typical; the higher pressure is necessary to squeeze liquid from the seal zone when splashing has occurred. A 50.8 µm LLDPE sealant is not normally specified for retort pouches requiring sustained 121 °C overpressure processing or for hot-fill above 80 °C; at those temperatures the seal may creep under headspace pressure and fail along the fin-seal edge. For pasteurized liquids up to 65 °C, it is suitable if seal strength after hot filling is verified by ASTM F88/F88M and the film is not exposed to free chlorine or strong oxidizing agents at elevated concentration. The main production failure in liquid pouch lamination is delamination caused by adhesive swelling when the packaged product contains surfactants or fatty acids. If the inner edge of the laminate is exposed at the seal cut, the product can wick into the foil-adhesive interface. Converters therefore specify a cut-edge quality with no exposed foil and verify bond strength after product contact by immersion testing at 40 °C for 21 days followed by ASTM F904 bond measurement. Because published data for this specific film under all liquid chemistries is limited, a product-laminate compatibility test is required before production.
| Process variable | Solventless adhesive lamination | Solvent-based adhesive lamination | Seal operation |
|---|---|---|---|
| Adhesive coat weight | 1.8–2.5 g/m² | 2.0–3.0 g/m² | — |
| Nip temperature | 60–75 °C | 70–85 °C | — |
| Cure | 48–72 h at 35 °C/50 % RH | 24–48 h at 45 °C | — |
| Surface energy | 38–42 mN/m | 36–40 mN/m | — |
| Seal temperature | — | — | 115–150 °C |
| Seal pressure | — | — | 276–483 kPa |
| Dwell | — | — | 0.3–1.0 s |
Household and institutional unit-dose sachets for fabric softeners, surface cleaners, and water-soluble active formulations employ 50.8 µm Sclairfilm GL-1 as the sealant web when the laminate is PET/foil/LLDPE or PET/LLDPE. The chemical resistance requirement in this sector is dominated by surfactant stress cracking, which can cause seal-area microcracks in low-density polyethylene but is less severe in linear low-density polyethylene because of its higher molecular-weight distribution and different branching architecture. Long-term compatibility is assessed by storing filled sachets at 40 °C and 65 % RH for 90 days and monitoring seal strength per ASTM F88/F88M, weight loss, and visual crazing. Formulations containing high levels of terpenes, aromatic solvents, or ketones can swell the polyethylene sealant and are outside the normal service envelope unless validated; the converter must request the complete liquid formulation because minor solvents can migrate through the seal layer. On high-output horizontal sachet lines, the sealant is expected to seal through a small degree of product contamination at the transverse seal, but no polyethylene film seals reliably through heavy foaming or through particulate residues. The 50.8 µm gauge is generally used for low-volume sachets; larger volumes may require a thicker sealant layer or a coextruded film with a high-toughness core. A second operational boundary is the presence of slip additives in the film: if the coefficient of friction rises above 0.35 on the seal side, feeding on vertical machines may become erratic, and the jam occurs at the forming collar rather than at the seal jaws.
When the 50.8 µm LLDPE web is run as the sealant side of a laminated reel on continuous-motion vertical form-fill-seal machines at speeds between 80 and 120 bags/min, the limiting property is no longer laminate bond strength but hot tack and surface friction. At those speeds, the bottom seal is subjected to product drop within milliseconds of jaw opening; if the hot-tack force is insufficient, the seal can unzip under the impact of product. Hot tack is measured by ASTM F1921 over the temperature range 105–150 °C; converter specifications for a 50.8 µm LLDPE sealant generally require a hot-tack peak above 2.0 N/15 mm within the seal initiation window, but the actual value depends on package fill weight and drop height. The sealant web is corona-treated on the adhesive side only; the opposite side is left untreated or lightly treated to maintain controlled slip. If the film is stored at temperatures above 35 °C or exposed to direct sunlight, slip additives can bloom unevenly, causing stick-slip behavior at the forming collar. Machine operators may compensate by opening the forming collar or reducing film tension, but this produces a wider back-seal overlap and higher reject rates. The correct remedy is to set the unwind tension on the film roll to 0.3–0.8 N/mm of web width and to maintain a dancer position near 50 % travel so that the LLDPE layer does not stretch under the intermittent pull of the draw-down belts. Drive rollers with rough surfaces can abrade the sealant and generate dust that contaminates the seal zone; smooth, clean, and temperature-controlled rollers are required. Thermal shock on high-speed lines occurs when the hot seal is immediately cooled by the product or by the chilled jaw cycle. If the cooling rate is too rapid, the LLDPE seal can develop internal stress at the seal interface, which reduces burst strength during subsequent drop tests. Production audits therefore include burst testing per ASTM F2054 and seal-strength testing per ASTM F88/F88M after 24 h, not just immediately after sealing. The seal jaws should be checked for temperature uniformity with a contact thermocouple across the entire seal width; a variation of more than ±3 °C at 130 °C setpoint indicates damaged heater cartridges or uneven jaw pressure that cannot be corrected by increasing the setpoint alone.
Among paper-based single-serve structures, 50.8 µm Sclairfilm GL-1 is placed as the innermost sealant web on paper/foil/LLDPE laminates used for sugar, instant coffee, salt, and dry creamer portion packs. The paper outer ply provides deadfold and surface printing; the foil mid-layer provides moisture and gas barrier; the LLDPE web contributes seal strength and prevents the paper edge from wicking moisture into the sachet. Seal operation for these portion packs is typically performed on high-speed stick-pack or sachet machines at 120–150 °C, 276–414 kPa, and dwell below 0.5 s. Because the paper layer insulates the seal interface from the heated jaw, the setpoint must be higher than in film-to-film structures, but the dwell cannot be extended without slowing the line. A quality check for paper/foil/LLDPE laminates is the measurement of seal strength after 24 h using ASTM F88/F88M; a minimum of 3.0 N/15 mm is common for portion packs filled with hygroscopic powder, but the limit is product-specific. If the foil layer contains pinholes, moisture ingress produces caking of the powder, and the failure is usually detected only after distribution; therefore incoming foil pinhole counts are specified. The 50.8 µm LLDPE layer alone provides little oxygen barrier, so non-foil paper/LLDPE laminates are limited to short-shelf-life products such as sugar or salt that tolerate moisture and oxygen exposure.
| Regulatory or test reference | Scope | Relevant test or condition |
|---|---|---|
| FDA 21 CFR 177.1520 | Olefin polymers for food contact | Food-type and migration limits per specific use condition |
| EU 10/2011 | Plastic food-contact materials | Overall migration ≤ 10 mg/dm² |
| ISO 11607-1 | Sterile barrier packaging | Seal and integrity validation |
| ASTM F88/F88M | Seal strength | Minimum validated per package configuration |
| ASTM F1921 | Hot tack | Seal window mapping |
| ASTM F1249 | Water vapor transmission rate | Barrier verification when foil or metallized web is used |
| ASTM D3985 | Oxygen transmission rate | Barrier verification for oxygen-sensitive structures |
| ASTM F2054 | Burst strength of flexible packages | Integrity under internal pressure |
Competitive DuPont™ Sclairfilm® GL-1 LLDPE Film, Laminating, 50.8 µm Thickness prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
DuPont™ Sclairfilm® GL-1 is a linear low-density polyethylene (LLDPE) film supplied in a nominal gauge of 50.8 µm and described by the manufacturer as a laminating grade. The web is produced from an ethylene/α-olefin copolymer and is intended for use as a component of multilayer flexible packaging structures rather than as a standalone printed or converted surface. Roll labels for this article generally identify the grade descriptor GL-1, the nominal thickness in micrometres, and the lot number. The grade is used in adhesive lamination, dry-bond lamination, and extrusion-laminated structures where seal strength, puncture resistance, and interlayer bond uniformity are process-critical.
Storage of the film in its original moisture-resistant wrap at ambient temperatures below 35 °C and relative humidity below 60% RH is standard practice. The film does not require pre-drying for moisture removal; however, condensation on roll edges should be prevented before corona treatment or adhesive coating. A first-in/first-out rotation period not exceeding 12 months from the mill roll date is commonly applied unless a new certificate of analysis indicates otherwise.
The principal distinction between GL-1 and a general-purpose LLDPE film lies in the surface engineering and additive package intended for laminating. A general-purpose LLDPE film may exhibit higher coefficient of friction, lower corona retention, or higher gel count, each of which can produce adhesive wetting defects, blocking in rewind, or visible lamination spots. The GL-1 designation identifies a laminating grade within the Sclairfilm® range, typically supplied with controlled slip and antiblock to allow unwind and rewind at production speeds without reducing adhesive anchorage. Published data for the exact additive formulation in GL-1 is limited to supplier-controlled disclosures; however, the functional consequence is reduction of blocking tendency and retention of film surface wetting above 38 dyn/cm as measured by ASTM D2578-09a.
Compared with a 50 µm cast LDPE laminating web, the linear polymer structure of GL-1 contributes higher tensile energy to failure and greater dart impact per unit gauge. The optical haze of a 50.8 µm LLDPE film is often marginally higher than that of an equivalent LDPE cast film, and the melt strength during extrusion coating is lower. These differences become relevant when a converter selects a web for a laminate requiring drop-load survival or puncture resistance against sharp-edged dry foods. Tensile properties are typically measured by ASTM D882-18 using 25.4 mm wide strips at a 500 mm/min crosshead speed after conditioning at 23 °C and 50% RH.
Compared with an ethylene-vinyl acetate sealant layer of equivalent gauge, the LLDPE chemistry of GL-1 does not introduce the acetic acid monomer by-products that can affect seal-bar contamination or taste and odour in sensitive dry foods. However, EVA sealant resins commonly initiate sealing at 80–95 °C, whereas LLDPE typically requires 100–120 °C. This higher sealing temperature may be a limitation in high-speed vertical form-fill-seal applications with short dwell times.
The values in Table 1 are class-typical reference ranges for a 50.8 µm LLDPE laminating film and are not contractual specification limits. Lot-specific certificate of analysis values and the supplier technical data sheet govern final release.
| Property | Unit | Reference range | Test method |
|---|---|---|---|
| Nominal thickness | µm | 50.8 ±10% | ISO 4593:1993 |
| Density | g/cm³ | 0.918–0.925 | ISO 1183-1:2019 |
| Tensile strength at break, MD | MPa | 25–40 | ASTM D882-18 |
| Elongation at break, MD | % | 500–800 | ASTM D882-18 |
| Dart impact | g | 150–400 | ASTM D1709-16a / ISO 7765-1 |
| Haze | % | 2–7 | ASTM D1003-13 |
| Gloss at 60° | GU | 70–90 | ASTM D2457-13 / ISO 2813 |
| Kinetic coefficient of friction | dimensionless | 0.15–0.60 | ASTM D1894-14 |
| Wetting tension after treatment | dyn/cm | 38–44 | ASTM D2578-09a |
| Seal initiation temperature | °C | 100–120 | ASTM F1921-20 |
Neither LLDPE nor LDPE provides a significant barrier to oxygen or water vapour. In a multilayer laminate, barrier is normally contributed by aluminium foil, metallized PET, PVdC-coated film, or EVOH. The GL-1 layer therefore functions as the sealant and mechanical toughening layer rather than a primary barrier component. The service temperature window is limited by the crystalline melting range of LLDPE, commonly 120–125 °C as measured by differential scanning calorimetry per ISO 11357-3. Continuous exposure above 80 °C is not recommended for dimensionally stable food-contact applications.
Before adhesive coating or laminating, the film surface should be verified with contact-angle dyne solutions using ASTM D2578-09a. A practical lower acceptance limit of 38 dyn/cm is common for solventless polyurethane systems; solvent-based primed systems can tolerate 36 dyn/cm but may produce more variable bond strength on high-speed lines. Corona discharge equipment operating at 1.5–3.0 kW per metre of web width and a line speed of 100–250 m/min can raise surface energy. Treatment beyond 46 dyn/cm may generate low-molecular-weight oxidized species that reduce interfacial bond strength and increase heat-seal contamination. Roll-to-roll handling after lamination is influenced by kinetic coefficient of friction; a very low slip package may induce telescoping on unsupported rewind, while an excessively high coefficient of friction can cause blocking in large-diameter rolls above 600 mm.
During blown-film extrusion of a laminating-grade LLDPE, a die gap of 1.5–2.5 mm and a blow-up ratio of 2.0–3.0 are typical. LLDPE requires higher extrusion pressure than LDPE because of its narrower molecular weight distribution and higher melt viscosity, commonly 10–25% higher pressure on a 63.5 mm grooved-feed extruder. Melt temperature is generally held between 190 °C and 230 °C to balance film optics and polymer degradation.
In dry-bond laminating, the web is combined with a secondary substrate such as biaxially oriented PET, oriented polyamide, or aluminium foil using a two-component polyurethane adhesive. Typical adhesive coat weights for film-to-film structures fall between 1.8 g/m² and 2.5 g/m² dry, applied by a gravure cylinder with a line screen of 140–180 lines/cm and a cell volume of 10–16 cm³/m². Nip temperature at the laminating station is commonly set at 50–60 °C with an associated nip pressure of 3–5 bar. Because LLDPE has higher elongation than LDPE at equivalent gauge, web tension during lamination should be reduced to 0.5–1.5 N/cm of web width; higher values can cause neck-in, misregister, and inconsistent final curl. The replacement of LDPE with LLDPE often permits a downgauging of 10–20 µm in the sealant layer because the dart impact and slow-puncture resistance of LLDPE are higher per unit thickness.
Laminate bond strength after 24 h room-temperature cure is commonly evaluated by ASTM F904-16. For an LLDPE/PET lamination with a solventless adhesive, cohesive failure in the adhesive or film yield typically occurs above 2.0 N/15 mm; values below 1.0 N/15 mm suggest inadequate surface treatment, amine blush, or incomplete cure. Hot-tack and heat-seal strength are measured per ASTM F1921-20 and ASTM F88/F88M-21. Seal-bar temperatures from 110 °C to 130 °C with a dwell of 0.5 s and a pressure of 2 bar are typical starting points for laboratory seal-curve determination.
Slitting of 50.8 µm LLDPE after lamination should use shear or razor slitting with blade geometry maintained to minimize edge stretching. Unwind tension is typically set at 0.3–0.8 N/cm for the laminate, and rewind taper from 40% to 20% of initial tension is used to prevent blocking and core crush on rolls above 400 mm outside diameter. Static elimination bars should be installed before the rewinder because LLDPE in dry conditions can retain charge densities above 5 kV, leading to dust pick-up and registration errors.
If a solvent-based polyurethane laminating adhesive is selected, the converter should verify solvent retention is below 5 mg/m² after the drying oven, because retained ethyl acetate or methyl ethyl ketone can swell the LLDPE surface and reduce interlayer peel strength. Oven temperatures segmented at 60 °C, 75 °C, and 85 °C with air velocity above 20 m/s are typical starting points; line speed is governed by the oven residence time needed to reach the target retention level.
Food-contact suitability for polyethylene homopolymers and copolymers is assessed under 21 CFR 177.1520(c), with migration limits specified in 21 CFR 176.170(c) or 177.1390(c) depending on the final laminate structure. In the European Union, a polyethylene sealing layer intended for contact with food is evaluated against Regulation EU No 10/2011, including an overall migration limit of 10 mg/dm² for food-contact plastics under worst-case intended use conditions. The film may also be included in declarations such as REACH SVHC absence and RoHS 2011/65/EU recast if supplied with supplier-issued attestation. Because GL-1 is supplied as a base film and not a converter-ready food-contact laminate, final compliance responsibility remains with the converter applying adhesives, inks, and secondary substrates.
| Standard or regulation | Applicability | Test or condition | Information source |
|---|---|---|---|
| 21 CFR 177.1520(c) | Olefin polymer food-contact use | Density, melting range, migration requirements | Supplier declaration |
| EU No 10/2011 | Food-contact plastic layers | Overall migration limit 10 mg/dm² | Converter validation |
| ASTM F904-16 | Laminate bond strength | Peel after cure | Incoming QC |
| ASTM F1921-20 | Hot-tack | Seal initiation and hot-tack window | Incoming QC |
| ASTM D2578-09a | Surface treatment | Dyne solution wetting | Incoming QC |
The film is not formulated as a high-temperature, retortable, or UV-stable grade. It should not be exposed to aromatic hydrocarbons, chlorinated solvents, or high concentrations of citrus oil during production trials because these agents can swell the polyethylene matrix and reduce mechanical properties. Corona treatment on both sides simultaneously is not recommended without monitoring of static charge, because backside treatment can lead to blocking in rewind. Published data for the specific configuration of GL-1 in high-barrier retort pouches is limited; validation should be performed on the actual lamination line and end-use packaging equipment.