| HS Code | 925366 |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Melt Index 190c 2 16kg | 0.75 g/10 min |
| Density | 0.918 g/cm³ |
| Melting Point | 122 °C |
| Vicat Softening Point | 95 °C |
| Tensile Strength At Yield | 10.3 MPa |
| Tensile Strength At Break | 24.1 MPa |
| Ultimate Elongation | 800% |
| One Percent Secant Modulus | 207 MPa |
| Dart Drop Impact | 120 g |
| Elmendorf Tear Strength Md | 240 g |
| Elmendorf Tear Strength Td | 480 g |
| Haze | 12% |
| Gloss 45 | 60 |
| Coefficient Of Friction | 0.15 |
| Slip | 1500 ppm |
| Antiblock | 2500 ppm |
As an accredited Dow Tuflin™ HS-7098E LLDPE factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Dow Tuflin™ HS-7098E LLDPE is supplied in 25 kg polyethylene-lined bags, palletized and stretch-wrapped for industrial transport. |
| Container Loading (20′ FCL) | 20′ FCL loading: Dow Tuflin™ HS-7098E LLDPE in 25 kg bags, palletized, approximately 20 MT total, 20 pallets per container. |
| Shipping | Dow Tuflin™ HS-7098E LLDPE is non-hazardous and not regulated for transport under DOT, IMDG, IATA, or ADR. Ship in original sealed bags or boxes on pallets. Keep dry, cool, and ventilated; avoid heat, sunlight, ignition sources, and strong oxidizers. Store away from food and feed. |
| Storage | Store Dow Tuflin™ HS-7098E LLDPE in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and oxidizing agents. Keep containers closed when not in use to prevent moisture, dust, and contamination. Protect from prolonged UV exposure and extreme temperatures. Follow first-in, first-out stock rotation. Store separately from incompatible materials. Use appropriate grounding and handling to avoid static buildup. |
| Shelf Life | Shelf life is typically 24 months from manufacture when stored unopened, dry, below 50°C, and away from direct sunlight. |
In heavy-duty shipping sack conversion, the outer layer formula is commonly composed of 70–80 wt% Dow Tuflin™ HS-7098E LLDPE and 20–30 wt% LDPE homopolymer to stabilize the bubble and maintain melt strength during low-neck-height film blowing. The blend is gravimetrically fed to a 75 mm single-screw extruder with a 30:1 L/D barrier screw and a feed throat held at 35–45 °C. Barrel zones climb from 180 °C to 215 °C, and the breaker plate carries a 20/40/60/20 mesh screen pack. Melt pressure at the screen pack is maintained below 320 bar, while die adapter melt temperature is controlled at 208–218 °C. The formulation is matched to the supplier certificate of analysis for melt index and density, because lot-to-lot drift in those values shifts bubble stance and gauge profile on sack film lines.
Film is produced on a three-layer blown film line with a 400 mm spiral mandrel die and a 2.2 mm die gap. Blow-up ratio is set at 2.8:1, and frost line height is held between 700 mm and 900 mm above the die face. Output reaches 280–320 kg/h when the middle-layer extruder is capped at 85% motor load. The tubular sheet is surface-treated to 38–42 mN/m for flexographic printing and converted on bottom-seal bag machinery into valve sacks or open-mouth sacks. Tensile properties are measured according to ISO 527-3 at 500 mm/min. At 150 µm gauge, quality specifications typically require dart impact of at least 800 g by ISO 7765-1 Method A and machine-direction Elmendorf tear above 10 N/mm by ISO 6383-2. For non-food industrial packaging, chemical compliance is limited to REACH Annex XVII restrictions and general heavy-metal limits; no direct food-contact clearance is claimed for this sack construction unless the converter qualifies the exact formulation under EU 10/2011 and FDA 21 CFR 177.1520.
Terminal products include 25 kg resin bags, mineral wool sacks, polymer granule sacks, lightweight aggregate packaging, and compressed insulation panel sleeves. On actual sack conversion lines, the main bottleneck is not extrusion output but bag-sealing consistency when the film contains high levels of lubricant or slip additive. Batch-to-batch variance in dart impact at 150 µm is reduced by limiting recycled core regrind to 20 wt% or less and by screening the regrind through a 2.0 mm mesh before re-introduction to the middle layer gravimetric feeder.
For black silage cover film, the exposed outer layer contains 6–8 wt% carbon black masterbatch and 0.5–1.0 wt% hindered amine light stabilizer concentrate let down into Dow Tuflin™ HS-7098E LLDPE. The concentrate carrier must be selected to match the melt flow of the virgin resin, because a carrier mismatch causes carbon black agglomerates in the bubble and pinholes after stress cracking. Dispersion is evaluated by ISO 18553 on 50 µm microtomed sections; agglomerates larger than 25 µm are rejected for outdoor exposure. The three-layer structure is black-white-black, with the white middle layer containing 8 wt% titanium dioxide concentrate and the inner black layer containing 5 wt% carbon black to reduce light transmission to the ensiled crop.
The line runs a 500 mm die with 2.5 mm die gap and 2.0:1–2.5:1 blow-up ratio. Melt temperature at the die is held at 200–220 °C, and film thickness is maintained at 150–200 µm. Corona treatment is not applied to the exposed surface because surface oxidation reduces weathering resistance and accelerates carbon black loss at the film surface. Weathering performance is tested by ISO 4892-2 cycle 1 for 3000 h. EN 13206:2017 provides the framework for tensile property retention and tear resistance of agricultural covering films after weathering. A converter must also confirm that the HALS package does not volatilize during extrusion above 220 °C; this is checked by production-run gel count and by retained stabilizer assay on the finished film.
Terminal downstream products include silage clamp covers, grain storage sheets, temporary onion storage covers, and baled silage overwrap. The failure mode observed on farm-stored covers is not tensile loss but folding fatigue at the clamp shoulder; repeated folding at −10 °C can crack the black layer if the outer film falls below 150 µm. Chemical compliance for this application is grounded in REACH Regulation (EC) No 1907/2006 Annex XVII; EU RoHS is not applicable to agricultural film. Carbon black masterbatch selected for silage covers should be free of polycyclic aromatic hydrocarbons above the relevant REACH restriction concentration, and the supplier declaration should identify the CAS numbers of the hindered amine stabilizer package.
On a cast stretch line running 25 µm hand-grade film, Dow Tuflin™ HS-7098E is metered into the core extruder at 60–70 wt% of the total web, with the outer cling layers carried by a low-density metallocene resin. The core blend comprises 85 wt% Tuflin™ HS-7098E and 15 wt% metallocene LLDPE to improve draw stability. Die gap is set at 0.8–1.2 mm, and the chill roll is held at 18–24 °C. Melt temperature at the die remains between 245 °C and 260 °C. Line speed is limited to 350–550 m/min depending on edge pinch stability and gauge uniformity. Pre-stretch ratio is normally kept at 180–220% for HS-7098E-rich core films, because the higher stiffness of this resin relative to metallocene-only grades raises unwind tension and makes deep pre-stretch beyond 250% prone to web breakage.
Puncture resistance is measured by ASTM D5748 at 250 mm/min; hand-grade 25 µm pallet wrap specifications commonly require a puncture force above 45 N for sharp-cornered loads. Machine-direction tensile break coefficient is measured by ASTM D882 at 500 mm/min. The cast line uses a 450 mm coat-hanger die with internal deckles; edge trim regrind is kept below 15 wt% because higher trim addition oxidizes the core and lowers puncture resistance. Terminal products include lightweight pallet stabilization wrap, corner-boarded panel wrap, and non-food secondary packaging wrap. If the wrap is used in indirect food-contact pallet overwrap, the converter must verify the exact construction under EU 10/2011 and FDA 21 CFR 177.1520; the cling layer additives are usually the limiting component, not the Tuflin™ HS-7098E core resin.
Extrusion coating of Dow Tuflin™ HS-7098E onto 70 g/m² kraft paper requires melt temperatures of 280–310 °C to promote adhesion and reduce viscosity during draw-down. The resin is processed neat or as an 80 wt% HS-7098E and 20 wt% low-melt-index LDPE blend to reduce neck-in and improve wetting on porous paper. Neutrally balanced coating-grade formulations are used without slip or antiblock unless the converter requires a coefficient of friction below 0.35 on the finished carton surface. The extruder is a 90 mm single-screw unit with 30:1 L/D, a coathanger die, and a 0.5 mm die gap. Air gap is set at 150–250 mm, and line speed is held between 120 m/min and 220 m/min. Neck-in is monitored at 25–50 mm per side; values above 60 mm per side indicate excessive degradation or an incorrect LDPE let-down ratio.
Adhesion to kraft paper is measured by ASTM D1876 T-peel at 300 mm/min, with target values between 2.0 N/15 mm and 4.0 N/15 mm depending on paper porosity and flame treatment. Coating weight is controlled to 15–25 g/m² by gravimetric scanner feedback; gauge variation at the die must stay within ±0.5 g/m² to avoid pinholes in subsequent flexographic printing. The terminal structures are frozen food carton liners, sugar stick pack overwrap, industrial sack barrier layers, and secondary liquid-packaging laminations. Compliance for food-contact coating is anchored to EU 10/2011 overall migration limit of 10 mg/dm² and to FDA 21 CFR 177.1520 olefin polymer clearance. The converter must verify specific migration limits for the coating additives and ensure that the paper substrate is food-contact approved for the intended temperature and time conditions.
| Downstream Use | Controlling Standard | Typical Verification Target |
|---|---|---|
| Heavy-duty sacks | ISO 7765-1 Method A | ≥ 800 g dart impact at 150 µm |
| Agricultural silage cover | ISO 4892-2 cycle 1 | ≥ 50% tensile retention after 3000 h |
| Cast stretch wrap core | ASTM D5748 | ≥ 45 N puncture at 25 µm |
| Extrusion coating | EU 10/2011 | ≤ 10 mg/dm² overall migration |
| Extrusion coating | FDA 21 CFR 177.1520 | Olefin polymer extractives per clause |
| Refuse sacks | EN 13592:2017 | Dart drop, dimensions, and tensile per sack class |
Where post-consumer LLDPE regrind exceeds 20 wt% in a refuse sack formulation, the virgin fraction based on Dow Tuflin™ HS-7098E is increased to preserve Elmendorf tear and dart impact after conversion. The film is blown on a 70 mm single-screw extruder with 30:1 L/D and a 300 mm die. Die gap is 1.8 mm, blow-up ratio is 3.0:1, and melt temperature is maintained at 190–210 °C. Film thickness ranges from 40 µm to 80 µm depending on sack capacity. The regrind is pre-dried below 0.05% moisture and screened through a 1.5 mm mesh before feeding; this removes gel precursors from the post-consumer fraction and reduces bubble instability at high frost line height.
Quality specifications for 50 µm can liner film typically require dart impact above 400 g by ASTM D1709 Method B and machine-direction Elmendorf tear above 800 g by ASTM D1922. Tensile strength at break is measured by ISO 527-3 at 500 mm/min. The finished sacks are tested to EN 13592:2017 for dimensions, dart impact resistance, and tensile strength. Heavy-metal restrictions follow the CONEG model legislation, US TPCH limits, and REACH Annex XVII. Slip and antiblock packages are held below 1500 ppm for the additive total to avoid lowering dart impact at downgauged 40 µm constructions. Terminal products include kitchen refuse sacks, refuse-derived fuel bags, recycling sacks, and commercial can liners for non-hazardous waste.
In smooth geomembrane fabrication, Dow Tuflin™ HS-7098E is extruded as a 0.5 mm to 2.0 mm sheet through a flat die with a width of 3–5 m. The resin is blended with 2.0–3.0 wt% carbon black masterbatch and 0.2–0.5 wt% antioxidant concentrate before entering a 120 mm single-screw extruder with 33:1 L/D. Melt temperature at the die is maintained between 220 °C and 240 °C. The sheet is calendered and cooled on polished rolls at 70–90 °C to relieve residual stress before edge trimming. Because this grade is not a high-molecular-weight geomembrane resin, the converter must validate stress crack resistance for the specific sheet thickness and field temperature range; published data for this specific configuration is limited.
Puncture resistance is measured by ASTM D4833 at 300 mm/min; a 1.0 mm smooth geomembrane specification often requires a puncture force above 400 N. Tensile properties are measured by ASTM D6392 or ISO 527-3 with a 50 mm gauge length. Carbon black dispersion is evaluated by ISO 18553 to ensure that agglomerates do not exceed 25 µm in the extruded sheet. The terminal uses include landfill caps, secondary containment liners, pond liners, and temporary canal liners. Chemical compatibility must be confirmed for the specific leachate, acid, or salt solution; general compliance is tied to national requirements for geosynthetic barriers, not to direct food-contact clearance.
Competitive Dow Tuflin™ HS-7098E LLDPE prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Dow Tuflin™ HS-7098E LLDPE is a linear low-density polyethylene resin supplied in pellet form for blown film extrusion. The nominal density is 0.926 g/cm³ measured by ASTM D1505-18, and the melt index is 0.95 g/10 min under ASTM D1238-20 at 190°C/2.16 kg. The resin is specified for heavy-duty sacks, industrial liners, agricultural films, and thick-gauge wrapping films where puncture resistance, Elmendorf tear strength, and stiffness are required in a single-layer or coextruded structure. Compared with a conventional butene-copolymer LLDPE of matched density and melt index, HS-7098E provides higher dart impact and tear strength at equivalent film gauge while maintaining a similar seal initiation range. The product is not supplied as a ready-to-use food-contact article; end-use compliance must be validated on the finished film structure.
The resin properties in the table below are determined on compression-moulded plaques or extruded film as indicated. Film values are representative for a 25 µm blown film produced on a single-screw extruder with a 30:1 L/D barrier screw, a 100 mm die diameter, a 1.2 mm die gap, a blow-up ratio of 2.5:1, and a die melt temperature of 210°C. These values are not direct specifications for finished commercial films because thermal history, die geometry, and frost line height shift the measured result.
| Property | Nominal value | Standard |
|---|---|---|
| Density | 0.926 g/cm³ | ASTM D1505-18 |
| Melt index, 190°C/2.16 kg | 0.95 g/10 min | ASTM D1238-20 |
| Tensile strength at break, machine direction | 41 MPa | ASTM D882-18 |
| Tensile strength at break, transverse direction | 32 MPa | ASTM D882-18 |
| Tensile elongation at break, machine direction | 600% | ASTM D882-18 |
| Tensile elongation at break, transverse direction | 750% | ASTM D882-18 |
| Dart drop impact, Type A | 170 g | ASTM D1709-22 |
| Elmendorf tear strength, machine direction | 450 gf | ASTM D1922-23 |
| Elmendorf tear strength, transverse direction | 550 gf | ASTM D1922-23 |
| Haze | 12% | ASTM D1003-21 |
| Gloss at 45° | 60 | ASTM D2457-21 |
Film properties generated on a high-stalk blown film line can differ from the tabulated values. If the die melt temperature is increased above 220°C, haze rises by 2% to 4% and dart impact can decline by 10% to 15%. If the frost line is lowered below 2.0 m, transverse direction tear improves but machine direction tear and stiffness decrease. Published data for this specific configuration is limited; the film producer should establish internal control limits on the actual production line.
On high-stalk blown film lines, HS-7098E is processed at melt temperatures between 190°C and 220°C. The low melt index of 0.95 g/10 min restricts mass output relative to higher-melt-index LLDPE grades. A 75 mm extruder operating at 60 rpm typically develops a melt pressure of 28 MPa to 35 MPa at the breaker plate. The primary limitation is not motor torque but bubble stability and the cooling capacity of the air ring. Raising melt temperature to increase throughput above the recommended window accelerates oxidative chain scission and reduces bubble strength. A higher-melt-index LLDPE of 1.5 g/10 min to 2.0 g/10 min can achieve higher throughput, but the gain is accompanied by lower dart impact measured by ASTM D1709-22 and lower Elmendorf tear measured by ASTM D1922-23.
In coextruded structures, HS-7098E is commonly placed in the core or outer layer of a three-layer film. The skin layers may use a metallocene LLDPE for seal performance or a high-pressure LDPE for melt strength. This configuration permits down-gauging while retaining the slow-crack-growth resistance and stiffness contributed by the HS-7098E layer.
Heavy-duty sack film at 100 µm to 150 µm is usually produced by blending 10% to 20% by weight of a high-pressure LDPE with a melt index of 0.5 g/10 min to 1.0 g/10 min. The LDPE improves bubble stability and heat-seal integrity. At 125 µm, blended film typically retains a dart impact above 300 g and an Elmendorf tear above 1,000 gf. Seal initiation temperature under ASTM F88/F88M-23 is generally 105°C to 110°C at a 0.5 s dwell time, but the exact value depends on corona treatment level, slip and antiblock loading, and the LDPE carrier.
HS-7098E is differentiated from butene-copolymer LLDPE film resins primarily by its short-chain branching distribution. The longer α-olefin comonomer increases the concentration of load-bearing tie chains in the amorphous phase, which raises dart impact and low-temperature toughness at equivalent density. In comparison with a butene-copolymer LLDPE of matched 0.926 g/cm³ density and 0.95 g/10 min melt index, machine-direction Elmendorf tear is typically 15% to 25% higher. Tensile yield strength remains within ±5% of the butene reference. Clarity may be slightly lower due to increased internal haze, while the hot-tack window is comparable. Published data for the specific competitive grade under identical extrusion conditions is limited; the comparison is based on class-level differences rather than a single commercial lot.
The processing difference is also measurable. Because the longer comonomer reduces crystalline uniformity, the resin has a broader melting range and a lower peak melting point than some high-stiffness butene grades. This broadening improves seal initiation but can narrow the bubble stability window on unsupported high-stalk lines. The resin is therefore less forgiving of sudden changes in frost line height than a general-purpose butene LLDPE of the same melt index.
Down-gauging agricultural bale wrap from 30 µm to 22 µm transfers the failure mode from tensile yielding to slow-rate puncture and tear propagation. Slow-rate puncture resistance under ASTM D5748-19 remains sufficient for dry hay baling when the film contains an appropriate cling agent and is processed at a blow-up ratio above 2.0:1. A loss of dart impact of more than 10% during down-gauging indicates that the frost line is too low or that the melt temperature has exceeded the recommended window.
The base resin does not contain a UV stabilizer package sufficient for multi-season outdoor exposure. Agricultural films that remain in the field for more than one season typically require 0.5% to 1.0% of a HALS/UV absorber masterbatch. Retained tensile elongation after 1,000 h of ASTM D4329-21 QUV exposure is the appropriate acceptance criterion; a retained elongation above 50% of the original value is commonly specified for silage wrap.
Extended residence time at melt temperatures above 230°C causes chain scission, gel formation, and a measurable loss of film impact. The antioxidant package is intended for short residence time in blown film extrusion, not for repeated heat histories. Film producers should limit the resin to 2 heat cycles and should not reprocess edge trim or start-up scrap at levels above 15% without verifying melt index by ASTM D1238-20 and dart impact by ASTM D1709-22. Amine-based antifog additives and nitrogen-containing slip agents can interfere with the phenolic stabilizer system; if such additives are required, oxidation induction time should be verified by ASTM D3895-19.
Storage of the pellet prior to extrusion is relatively insensitive to moisture. Pre-drying is not normally required unless the resin has been stored at relative humidity above 60% RH, in which case drying at 60°C to 70°C for 2 h removes surface moisture and prevents bubble formation at the die. Contact compliance for food packaging is referenced to 21 CFR 177.1520(c) 3.2(a); European food-contact assessment is referenced to EU Regulation 10/2011. Heavy-metal restrictions for packaging are assessed under RoHS Directive 2011/65/EU and REACH Annex XVII. The raw resin is not supplied with a USP Class VI certificate unless the finished article is validated separately.