| HS Code | 528689 |
| Product Name | Dow TUFLIN™ HS-7046 NT 7 Linear Low Density Polyethylene Resin |
| Manufacturer | Dow |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene-1 |
| Density | 0.918 g/cm³ |
| Melt Index 190 C 2 16 Kg | 1.0 g/10 min |
| Melting Point | 122 °C |
| Vicat Softening Point | 100 °C |
| Tensile Strength At Yield | 11 MPa |
| Tensile Strength At Break | 22 MPa |
| Elongation At Break | 700% |
| Flexural Modulus | 240 MPa |
| Dart Drop Impact | 120 g |
| Elmendorf Tear Strength Md | 250 g |
| Elmendorf Tear Strength Td | 400 g |
| Haze | 10% |
| Gloss 45 | 60% |
As an accredited Dow TUFLIN™ HS-7046 NT 7 Linear Low Density Polyethylene Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Typically packaged in 25 kg polyethylene bags, 40 bags per pallet (1,000 kg); bulk options available. |
| Container Loading (20′ FCL) | 20′ FCL container loading: Dow TUFLIN™ HS-7046 NT 7 Linear Low Density Polyethylene Resin, 25 kg bags, palletized, shrink-wrapped, secured. |
| Shipping | Dow TUFLIN™ HS-7046 NT 7 is shipped as non-hazardous LLDPE pellets in 25-kg bags, octabins, or bulk trucks/railcars. No UN number, hazard class, or special transport label is required. Keep dry, clean, and protected from UV; avoid excessive heat and bag damage. |
| Storage | Store in a cool, dry, well-ventilated area, away from direct sunlight, heat, sparks, and open flames. Keep bags or containers closed, clean, and dry, raised off the floor on pallets. Avoid moisture, dust, and contamination. Use moderate ambient temperatures and prevent prolonged UV exposure. Follow good housekeeping and first-in, first-out stock rotation, plus the manufacturer’s safety data sheet. |
| Shelf Life | Typically 24 months from manufacture when stored unopened in original packaging, cool, dry, and away from direct sunlight. |
In heavy-duty shipping sack and FIBC liner manufacturing, Dow TUFLIN™ HS-7046 NT 7 is processed as the primary load-bearing layer at 80–100 wt%, with 0–20 wt% LDPE added as a bubble-stability and draw-down modifier and 2.5–4.0 wt% carbon black masterbatch incorporated when ultraviolet shielding of the packaged product is specified. Compliance for non-dangerous-goods flexible intermediate bulk containers references ISO 21898:2004; where inner liners are used within UN-certified bags, converter testing follows the UN 13H2 protocol for dangerous goods containment. Downstream blown-film conversion typically uses a grooved-feed single-screw extruder of 75–90 mm barrel diameter and 30:1 L/D, feeding a die with diameter 250–350 mm and die gap 1.2–1.6 mm, run at blow-up ratio 2.2:1–2.8:1 and melt temperature 190–210°C. Terminal product types include sewn open-mouth sacks, pinch-bottom sacks, valve sacks, and insert liners for bulk bags rated at 500–1,500 kg.
| Property | Method designation | Use in converter release |
|---|---|---|
| Dart drop impact | ASTM D1709-22 | Fill-line drop survival |
| Elmendorf tear | ASTM D1922-23 | Gusset tear resistance |
| Tensile strength at break | ASTM D882-18 | Load-bearing capacity |
| Melt mass-flow rate | ISO 1133-1:2022 | Extruder output verification |
Melt fracture becomes observable on these lines when die-lip shear rate exceeds 1,000–1,200 s⁻¹ or when die temperature drops below 180°C; the resulting sharkskin texture reduces dart impact retention and increases printing reject rates on multi-wall sacks. Pressure fluctuation at the screen changer greater than ±8 bar typically produces gauge bands with a periodicity corresponding to screw speed, which converts into low tear resistance at gusset creases. Converter acceptance for a 125 µm monolayer heavy-duty sack film is assessed with ASTM D1709-22 Method A, ASTM D1922-23, and ASTM D882-18; tensile strength at break is commonly specified at ≥25 MPa in the machine direction, and elongation at break above 400% is used as the release threshold. Published converter release values for this specific resin configuration are limited; final acceptance is therefore confirmed through fill-line drop trials and bag compression tests using converter-defined protocols.
Carbon black masterbatch additions above 4.0 wt% reduce dart impact retention below 80% because dispersed agglomerates act as stress concentrators; below 2.5 wt%, ultraviolet shielding is insufficient for outdoor-stored sacks. No predrying is required at ambient relative humidity below 60%; surface condensation from cold warehouse storage must be removed by a hot-air knife at 50–60°C before feeding. Regrind from heavily wax-lubricated HDPE films is incompatible in high-load formulations because wax migration to the seal zone can lower weld strength during bottom sealing. Bubble instability is controlled by maintaining frost-line height at ±30 mm of the set point; excursions beyond this range change transverse direction tear and cause flapping at the collapsing frame.
Agricultural silage-cover and clamp-film conversion places the resin in a three-layer coextruded structure at 70–85 wt% in the load-bearing core and 60–80 wt% in the outer weathering layer, the balance being LDPE, 6–12 wt% UV/HALS masterbatch, and 2–4 wt% anti-fog masterbatch where condensation control is required. Compliance is tested against EN 13206:2017 for thermoplastic agricultural films; weathered tensile and elongation are measured according to EN ISO 527-3, and outdoor exposure is correlated through ASTM G154 fluorescent-UV weathering with UVA-340 lamps at 0.89 W/(m²·nm) irradiance. Downstream processing runs on three-layer blown-film lines with a 250–350 mm die, die gap 1.4–1.8 mm, blow-up ratio 2.0:1–2.5:1, frost-line height 400–600 mm, and reel widths up to 3,000 mm. Terminal products include silage clamp covers, round bale wrap films, greenhouse side sheets, and agricultural fumigation films in thicknesses from 100 µm to 250 µm.
When the UV/HALS masterbatch addition in the outer layer is raised above 12 wt%, interlayer peel strength drops because hindered amine stabilizer exudation at the interface disrupts chain entanglement. Below 6 wt%, retained elongation after weathering falls below multi-season requirements under EN 13206:2017. A production bottleneck occurs with frost-line height variation greater than ±30 mm; transverse gauge bands develop and low-temperature dart impact under ASTM D1709-22 Method A becomes non-uniform across the web. Surface condensation during winter conversion requires predrying of masterbatch at 50–60°C for 4–6 h when ambient RH exceeds 60%.
Because heat-seal strength after filling at −40°C controls material selection in frozen-food film, Dow TUFLIN™ HS-7046 NT 7 is introduced at 70–85 wt% with 15–30 wt% LDPE to raise bubble stability; slip and antiblock additives are dosed at 500–1,000 ppm erucamide and 2,000–5,000 ppm synthetic silica, respectively. Food-contact compliance is established under FDA 21 CFR 177.1520(a)(3)(i) and EU Regulation (EU) No 10/2011, with migration testing according to EN 1186-1 and specific migration limits for slip additives controlled by the converter. Downstream conversion uses a 65–75 mm grooved-feed extruder with 30:1 L/D, die gap 1.4–1.8 mm, blow-up ratio 2.0:1–2.4:1, and film thickness 40–80 µm. Terminal products include frozen vegetable pillow packs, frozen seafood film, ice-pack pouches, and overwrap for frozen bakery items.
The resin is not an oxygen-barrier resin; when shelf life beyond 30–45 days is required, a coextruded EVOH or PVdC structure is specified. Low-temperature dart impact should be measured after conditioning at −20°C for 24 h according to ASTM D1709-22, because ambient-temperature results do not predict failures in blast-freezer fill lines.
In extrusion lamination and adhesive-laminated flexible packaging, the resin is compounded into the sealant web at 20–35 wt%; the remaining fraction is LDPE, with antiblock at 3,000–6,000 ppm synthetic silica and slip at 400–800 ppm erucamide when coefficient of friction below 0.25 is required on high-speed vertical form-fill-seal lines. Food-contact compliance for sealant layers follows FDA 21 CFR 177.1520 and EU Regulation (EU) No 10/2011; for retortable structures, lamination bond strength is verified after 121°C retort by ASTM F904-98(2021). Downstream cast-film or blown-film conversion produces a 30–60 µm web, which is subsequently corona-treated to 38–42 mN/m and adhesive-laminated to PET, aluminum foil, or metallized OPP. Terminal products include stand-up pouches, four-side-seal sachets, lidding films, and retort pouch sealant layers.
Hot-tack is measured by ASTM F1921; seal initiation temperature shifts upward by 3–5°C for every 10 wt% LDPE addition. Slip migration into the seal layer reduces hot-tack if erucamide exceeds 800 ppm; therefore, converters running retort pouches cap slip at 400 ppm and raise antiblock instead. A process boundary occurs when corona treatment exceeds 44 mN/m: surface oxidation can create polar species that reduce hot-tack initial bonding. CoF kinetic values are checked with ISO 8295:1995; for high-speed filling, kinetic COF below 0.20 is typical.
Extrusion coating of liquid-paperboard and sachet base stock blends the resin at 20–40 wt% into LDPE to raise tear resistance without exceeding the draw-down limits of a 90 mm extruder with 30:1 L/D, deckled die width 1,500–2,500 mm, and coating speed 150–300 m/min. Compliance for direct food-contact coatings is established under FDA 21 CFR 177.1520 and EU Regulation (EU) No 10/2011; adhesion to paperboard is checked by cross-cut tape testing under ASTM D3359-23 and hot-tack by ASTM F1921. Downstream process melt temperatures are 280–300°C at the die, chill-roll temperature 10–15°C, coating weight 15–30 g/m², and nip pressure maintained at 3–5 N/mm². Terminal product types include liquid-paperboard cartons, sugar and salt sachets, medical lidding coated base stock, and barrier overwrap for dry powders.
Draw resonance develops at coating speed beyond 300 m/min when LLDPE content exceeds 40 wt% because the melt elasticity of the blend drops; neck-in increases from 30 mm to 60 mm depending on die width and melt temperature. Printed paperboard with residual moisture above 6% must be predried before coating to avoid steam pinholes at the chill-roll nip. Die-lip buildup from low-gel failures is controlled by maintaining a die gap of 0.5–0.8 mm and using a purge of 5 kg to 10 kg LDPE between product changes.
Machine-stretch film conversion doses the resin at 70–85 wt% in the core layer, with 15–30 wt% metallocene LLDPE as a modifier and 1.5–3.0 wt% polyisobutylene tackifier in the cling layer; edge layers are formulated at lower cling to avoid blocking. Compliance for industrial palletizing is not food-contact; mechanical acceptance is controlled by ASTM D5748-23 puncture propagation, ASTM D882-18 tensile properties, and ASTM D5459-22 elastic recovery. Downstream cast-film lines use a 75–120 mm extruder, 2,000–3,000 mm die width, 0.8–1.2 mm die gap, chill-roll temperature 18–25°C, and line speeds up to 400 m/min. Terminal products include machine stretch film for A-type pallet wrappers, rotary arm wrappers, and hand-stretch film in thicknesses 12–23 µm.
At pre-stretch ratios above 300%, the film enters the strain-hardening plateau and puncture resistance falls nonlinearly; converter trials indicate that 250% is a practical upper limit for this resin unless a metallocene-rich outer layer is used. Blocking force above 30 g as measured by ASTM D3354-15 can interrupt high-speed unwinding at 200 m/min. When the chill-roll temperature exceeds 25°C, the cling layer develops plate-out on the roll surface within 12 h of continuous operation, requiring a 15 min shutdown for roll cleaning.
Competitive Dow TUFLIN™ HS-7046 NT 7 Linear Low Density Polyethylene Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Dow TUFLIN™ HS-7046 NT 7 is a pelletized linear low density polyethylene resin in which the polymer backbone is produced with a controlled short-chain branch distribution characteristic of a solution polyethylene process. The publication-grade nominal density is 0.918 g/cm³ when measured according to ISO 1183-1:2019, and the nominal melt flow rate is 0.90 g/10 min at 190°C and 2.16 kg when measured according to ISO 1133-1:2022. The “NT 7” suffix identifies a particular stabilizer and pellet-handling package; the current supplier data sheet should be consulted to establish whether a slip or antiblock additive is present, because this variable alters film coefficient of friction and blocking force in wound rolls. The resin is positioned in the heavy-duty film segment rather than in thin commercial overwrap, because its melt flow rate and density favor bubble stability at intermediate throughput while retaining the toughness required in industrial liners, carrier film, and agricultural overwrap. For material selection, the grade is classified as an LLDPE film resin; it is not sold as an injection molding or rotational molding grade, and published data for these processes are limited. Because the melt flow rate is a single-point viscosity indicator, converters requiring shear sensitivity should request a melt flow ratio or dynamic viscosity measurement under ISO 6721-10 before line start-up.
Film impact on a 45 mm blown film line is controlled less by cylinder temperature than by die gap, frost line, and bubble geometry. For this density and melt flow rate class, the die exit melt temperature is commonly maintained at 193–232°C, with higher settings used only when line speed must be increased above the normal range. Typical parameters for a single-layer film structure are shown in the following table.
| Melt temperature at die exit | 193–232°C | Infrared probe at die lip |
| Blow-up ratio | 2.0–3.0 | Bubble geometry, single-layer film |
| Die gap | 1.8–2.5 mm | Annular lip |
| Frost line height | 300–900 mm | Measured from die face |
| Extruder L/D | 24:1–30:1 | Smooth-bore barrel with mixing section |
Dart impact is quantified by ASTM D1709 or ISO 7765-1:2022 on 25 μm film; Elmendorf tear is quantified by ASTM D1922 or ISO 6383-2:2023. Tensile property comparisons are performed under ASTM D882 at a crosshead speed of 500 mm/min. A reduction in melt temperature within the specified range, combined with a higher frost line, tends to preserve molecular orientation and dart impact, but frost-line adjustment beyond 900 mm on low-capacity air rings can reduce film flatness and gauge uniformity. On production-scale lines, the practical upper limit for stable bubble diameter is set by air ring cooling capacity; if the bubble circumference oscillates above ±5 mm, the gauge band can exceed ±8% and localized weak spots may fail dart impact testing. Because LLDPE has lower melt strength than high-pressure LDPE, older single-lip air rings commonly require addition of 5–15 wt% LDPE to stabilize the bubble before a dual-lip air ring or internal bubble cooling system is available.
Food-contact status for film produced from this resin is determined on the finished article, not on the pellet alone. In the United States, olefin polymers may be covered under 21 CFR 177.1520(c) 3.1a for low-temperature use, but the applicable paragraph depends on food type, extractive limits, and temperature. Under EU Regulation (EU) No 10/2011, overall migration must not exceed 10 mg/dm² for the finished article when tested with the prescribed food simulant. The converter should obtain the supplier’s regulatory certificate and, for high-fat simulants D1 or D2, request specific migration data. The following matrix identifies the principal frameworks applied to finished polyolefin articles.
| U.S. food contact | 21 CFR 177.1520(c) 3.1a | Finished article, end-use conditions |
| EU food contact | Overall migration ≤ 10 mg/dm² | EU Regulation (EU) No 10/2011, simulant specified by food type |
| REACH | SVHC ≤ 0.1 wt% | Regulation (EC) No 1907/2006, Article 33 |
| RoHS | Lead ≤ 1000 mg/kg, mercury ≤ 1000 mg/kg, cadmium ≤ 100 mg/kg | Directive 2011/65/EU Annex II, homogeneous material |
Pellets are non-hygroscopic; no drying is required for routine blown film, but surface condensation on cold pellets entering a warm building above a dew point of 18°C can be removed by a 70°C hopper dryer for 2 h if bubble pinholes are observed. Where coefficient of friction below 0.25 is required, slip/antiblock masterbatch is added at the throat at 2–5 wt%; migration rate is affected by film thickness, storage temperature, and additive solubility in the amorphous fraction of the film.
Low seal initiation is an expected property for LLDPE of 0.918 g/cm³ density relative to high-pressure LDPE, because the melting range is broadened by the short-chain branch distribution. Seal performance is not fixed by the pellet alone; it depends on gauge, seal bar pressure, dwell time, and additive migration. A laboratory heat-sealing protocol using ASTM F1921-12 is used to generate hot-tack curves, while seal strength is measured by ASTM F88/F88M-21. Published data for this specific HS-7046 NT 7 film configuration is limited; converters routinely establish minimum seal temperature on their own equipment using a dwell time of 0.5 s and a pressure of 0.40 MPa. In a coextruded structure, this resin is used as a sealant layer with an LDPE or ionomer core; it is not recommended for seal temperatures exceeding 150°C because oxidative tack and off-odor may occur. For sustained high-temperature seals, an ethylene-vinyl acetate or ionomer sealing layer should be substituted, and seal compatibility should be tested under ASTM F2029 or the applicable film-seal curve specification.
Compared with general-purpose butene-based LLDPE of comparable melt index, a longer α-olefin comonomer increases tie-molecule concentration at equivalent crystallinity, which typically translates into higher Elmendorf tear and dart impact in 25 μm blown film. This advantage cannot be assumed without film fabrication; die gap and cooling rate are strong secondary variables. In comparison with high-pressure LDPE, HS-7046 NT 7 exhibits lower melt strength; therefore, bubble stability on single-lip air rings older than 20 years may require 5–15 wt% LDPE addition or a dual-lip air ring with internal bubble cooling. The resin is used in applications in which the finished article must tolerate puncture, stress cracking, and repeated flexing rather than high stiffness; a tensile modulus value below 260 MPa in the machine direction is typical for films in this density class under ASTM D882, but exact values must be taken from the supplier certificate. Environmental stress-cracking resistance is characterized by ASTM D1693 or ISO 22088-1, though published data for this specific film grade are limited. In one typical converting sequence, a heavy-duty industrial liner is down-gauged from 50 μm to 38 μm and retains falling dart impact if the bubble is cooled with a frost line below 900 mm and the die gap is held at 2.0 mm. The downgauging benefit is not uniform across all gauges; below 20 μm, tear propagation resistance can become more sensitive to trim orientation and creasing in high-speed bag conversion.
Surface moisture, not absorbed moisture, is the principal cause of bubble instability in this non-hygroscopic resin. On a 55 mm grooved-feed extruder running at 120 kg/h, cold pellets transferred from an unheated silo into a 28°C and 60% relative-humidity mezzanine can condense enough water to produce micro-voids and visible pinholes in 25 μm film. The resulting defects are commonly misdiagnosed as melt fracture; the differential diagnosis is made by observing a decline in melt pressure fluctuations after hopper residence. When surface condensation is suspected, prewarming pellets to 20°C or applying dehumidified conveying air with a dew point below −20°C is more effective than extended drying. No separate predrying stage is required under typical indoor storage conditions below 60% relative humidity. Melt temperature should remain below 260°C; prolonged hold-up in the die or adapter above that threshold can generate oxidized gel particles and brown specks in film. On a single-screw line, the barrel profile is typically set with a reverse temperature gradient, from 180°C in the feed zone to 215°C at the metering zone, to increase shear heating and melt uniformity without exceeding 240°C at the front zone. If a line must be shut down for more than 20 min, the die and adapter should be kept at a reduced temperature rather than left at full operating setpoint.
Because the stabilizer package is formulated for extrusion at 193–232°C, repeated regrind levels above 30% can shift viscosity and gel content. If a high-gloss surface is required, a lower-viscosity LDPE blending partner is usually selected; addition of perfluorinated processing aids above 0.1 wt% may alter seal performance. The resin is compatible with typical polyolefin masterbatches and regrind streams; it is not compatible with condensation polymers such as PET or polyamide in a melt blend, though coextruded structures with tie layers are common. Acidic or amine-based additives should be evaluated for interaction with the stabilization system before dry-blending. For film structures requiring UV resistance, a hindered amine light stabilizer masterbatch is normally added at 2–4 wt%, but the addition level must be verified by accelerated weathering under ISO 4892-2:2024 for the intended service environment. Published data for this specific HS-7046 NT 7 configuration in rotational molding, injection molding, or profile extrusion is limited; use of the resin outside blown or cast film converting should not proceed without a feasibility trial.