| HS Code | 321944 |
| Productname | Dow FINGERPRINT™ DFDA-7510 NT Linear Low Density Polyethylene Resin |
| Polymertype | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene |
| Density | 0.920 g/cm³ |
| Meltindex 190c 2 16kg | 0.75 g/10 min |
| Meltflowratio I21 I2 | 27 |
| Vicatsofteningpoint | 95 °C |
| Meltingpoint | 121 °C |
| Tensilestrengthatyield Md | 10.3 MPa |
| Tensilestrengthatbreak Md | 27.6 MPa |
| Elongationatbreak Md | 700% |
| Dartdropimpact | 200 g |
| Elmendorftear Md | 250 g |
| Elmendorftear Td | 450 g |
| Haze | 12% |
| Gloss 45deg | 60 |
| Antiblock | None |
| Slip | None |
As an accredited Dow FINGERPRINT™ DFDA-7510 NT Linear Low Density Polyethylene Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Typically packaged in 25 kg bags or 1,000 kg bulk bags, and also supplied in industrial bulk trucks or railcars. |
| Container Loading (20′ FCL) | 20′ FCL: Dow FINGERPRINT™ DFDA-7510 NT LLDPE resin in palletized 25 kg bags, stretch-wrapped, secured for ocean transport. |
| Shipping | Dow FINGERPRINT™ DFDA-7510 NT Linear Low Density Polyethylene Resin is shipped as a non-hazardous solid in 25 kg bags, bulk bags, or bulk containers. It is not regulated for DOT, IMDG, or IATA transport. Protect from moisture, heat, and contamination; keep packaging closed during handling and storage. |
| Storage | Store Dow FINGERPRINT DFDA-7510 NT resin in a cool, dry, well-ventilated area, away from direct sunlight, heat, and ignition sources. Keep original packaging sealed to prevent moisture and contamination. Avoid contact with strong oxidizing agents. Use first-in, first-out rotation. Protect from UV light and dust accumulation. Do not store outdoors unless fully protected. Consult the SDS for detailed guidance. |
| Shelf Life | Shelf life: typically 24 months from manufacture when stored unopened in a cool, dry, well-ventilated area away from direct sunlight. |
On a 60 mm single-screw blown-film line with L/D 25:1–30:1 and dual-lip air ring, DFDA-7510 NT is metered in the core and skins at 60–85 wt%, LDPE at 10–30 wt%, and carbon black masterbatch at 2–4 wt% where opacity and ultraviolet resistance are specified. Regulatory compliance for industrial chemical sacks is anchored to REACH Regulation (EC) No 1907/2006 article obligations; when the sack is used for dry bulk food ingredients under incidental contact, the food-contact layer must meet 21 CFR 177.1520(c) 3.2a or Regulation (EU) No 10/2011 with overall migration not exceeding 10 mg/dm² by EN 1186. Converter lot acceptance requires a certificate of analysis for melt mass-flow rate under ISO 1133-1:2022 at 190 °C and 2.16 kg, and density under ASTM D792.
The dominant processing boundary is the interaction between frost-line height and die-end pressure. With a die gap of 1.8–2.5 mm and blow-up ratio 2.5:1–3.2:1, melt temperature is maintained at 195–215°C; below 190°C, the higher shear viscosity of LLDPE raises die pressure and motor load, and sharkskin melt-fracture can appear at extrusion rates above 85–100 kg/h. Above 215°C, oxidation products deposit on the die lip and cause bubble strike-through. Frost-line height is kept between 45 cm and 75 cm from the die face, and the collapsing frame angle is held below 25° to prevent edge creasing. On high-output heavy-duty sack lines, gusset-fold gauge variation is observed at ±8–12% unless the air ring is shimmed for edge bead compensation.
Where high dart impact and Elmendorf tear are required, DFDA-7510 NT is charged toward 80–85 wt%; the LDPE portion should not be reduced below 10 wt% because the bubble loses elastic stability at blow-up ratios above 3.0:1. Filler addition is limited to 5 wt% or less because calcium carbonate increases blocking at the nip and lowers tear. Terminal products include 50–200 µm heavy-duty shipping sacks, construction waste sacks, powder chemical liners, and kraft paper sack film lamination substrates.
Vertical form-fill-seal lines running at 40–70 cycles/min impose a seal jaw residence time of 0.3–0.8 s, making hot-tack strength and seal initiation temperature more critical than long-time seal strength. DFDA-7510 NT is let down at 70–80 wt% with LDPE at 10–20 wt% and a slip/antiblock masterbatch at 1–3 wt%; the final film erucamide level is held at 400–800 ppm because lower levels block sealing jaws and levels above 800 ppm suppress hot-tack by surface bloom. Compliance is anchored to 21 CFR 177.1520(c) 3.2a for olefin polymers in contact with frozen aqueous and fatty foods under conditions E–G, Regulation (EU) No 10/2011 with overall migration ≤10 mg/dm² by EN 1186, and GB 4806.7-2016 for food-contact plastic materials. The production route is blown film on a 45–65 mm extruder with L/D 25:1–28:1, die gap 1.5–2.0 mm, blow-up ratio 2.2:1–2.8:1, and film thickness 30–80 µm; the web is printed, slit, and mounted on vertical form-fill-seal machines. Terminal products include frozen vegetable pouches, IQF seafood bags, frozen bakery films, and ice cream multipack films. The operational limit is reclaim contamination: PVdC or nitrile barrier scrap must not enter the DFDA-7510 NT reclaim stream because incompatible melting and localized acid release generate pinholes and reduce hot-tack.
| Downstream route | Jurisdiction/region | Standard or test method | Required or measured boundary |
| Heavy-duty sack | EU | REACH Regulation (EC) No 1907/2006 | Article obligations; SVHC declaration when required |
| Heavy-duty sack, dry food incidental contact | US FDA | 21 CFR 177.1520(c) 3.2a | Extractive conditions A–H; lot certificate required |
| Frozen food form-fill-seal | EU | Regulation (EU) No 10/2011, EN 1186 | Overall migration ≤10 mg/dm² |
| Frozen food form-fill-seal | China | GB 4806.7-2016 | Food-contact plastic material migration limits |
| Agricultural silage film | EU | EN 13207:2001 | Tensile and tear after weathering storage |
| Geomembrane sheet | International | GRI-GM17 | ESCR, thickness tolerance, carbon black dispersion |
| Kraft paper lamination | US FDA | 21 CFR 176.170, 21 CFR 177.1520 | Paper and polymer component food-contact conditions |
| Chemical drum liner | EU/US | REACH Regulation (EC) No 1907/2006, 21 CFR 177.1520 | Chemical resistance; food contact when applicable |
Production of silage clamp and stretch tube structures uses DFDA-7510 NT at 70–90 wt% in the core, HDPE or LDPE at 10–25 wt% for film stiffness, and a UV masterbatch at 3–6 wt%; black silage film incorporates carbon black at 2–4 wt%. The applicable product standard is EN 13207:2001 for thermoplastic silage films and tubes; tensile properties are measured under ISO 527-3, tear under ISO 6383-2, and oxygen transmission under ASTM D3985 at 23 °C and 0% RH. The process is blown film extrusion with melt temperatures of 190–215°C, blow-up ratio 2.0:1–3.0:1, die gap 1.8–2.4 mm, and thickness 100–250 µm. Terminal products include silage bags, clamp covers, stretch silage tubes, and round bale wrap backsheets.
The failure mode in this application is not ultraviolet loss alone but the acid condensate and bio-derived leachate that collects at the film-soil interface. If the HDPE fraction is omitted or the UV package is poorly dispersed, stress cracking at the fold crease can occur before the 12-month storage cycle ends. UV active content is typically 0.3–0.8 wt% in concentrate form; total masterbatch above 6 wt% overloads the mixing section and produces surface bloom that lowers film-to-film friction. Converters pre-mix DFDA-7510 NT with UV concentrate in a low-speed tumbler for 10–15 min and monitor screw amperage to detect dispersion loss.
Stretch hood installations operating at 80–120 pallets/h require film recovery force after 55–70% elongation to remain above 8–12 N/50 mm on the pallet corner, while the film must avoid tearing over bagged irregular materials. DFDA-7510 NT is blended at 75–90 wt% with LDPE at 5–15 wt% and a cling or low-slip additive at 0.5–2 wt%; anti-block is omitted because high cling is required for pallet stability. Compliance falls under REACH Regulation (EC) No 1907/2006 and, for food-contact pallet hoods, Regulation (EU) No 10/2011; mechanical verification can use ASTM D882 for tensile recovery and ASTM D5748 for cling stretch film performance. The production route is triple-layer blown or cast extrusion with die gap 0.8–2.0 mm for cast and 1.5–2.5 mm for blown, at total thickness 60–150 µm; pre-stretch above 70% accelerates permanent set and lowers recovery force. Terminal products include stretch hoods for bagged cement, polymer granules, glass wool, beverages, and palletized chemical sacks.
| Downstream line | DFDA-7510 NT loading | Co-resins/additives | Critical processing boundary |
| Heavy-duty sack blown film | 60–85 wt% | LDPE 10–30 wt%, carbon black 2–4 wt% | Melt temperature >215°C causes lip oxidation; <190°C raises die pressure |
| Frozen food form-fill-seal | 70–80 wt% | LDPE 10–20 wt%, slip/antiblock 1–3 wt% | Erucamide >800 ppm suppresses hot-tack |
| Silage film | 70–90 wt% | HDPE/LDPE 10–25 wt%, UV 3–6 wt% | Total masterbatch >6 wt% causes surface bloom |
| Stretch hood | 75–90 wt% | LDPE 5–15 wt%, cling 0.5–2 wt% | Pre-stretch >70% accelerates permanent set |
| Geomembrane sheet | 85–100 wt% | Carbon black masterbatch 1.5–3.0 wt% | Melt temperature >230°C reduces ESCR |
| Drum liner | 65–85 wt% | LDPE 10–20 wt%, slip 0.5–1.5 wt% | Pinhole frequency at 100–250 µm |
| Kraft paper lamination | 90–100 wt% | LDPE 0–10 wt% | Melt residence >6–8 min reduces adhesion |
Flat-die extrusion of LLDPE geomembrane from DFDA-7510 NT requires a melt temperature of 200–230°C, die gap 2.0–3.0 mm, and beta or laser gauge scanning to hold thickness within ±5% or ±0.05 mm, whichever is larger. The formulation charges DFDA-7510 NT at 85–100 wt% with carbon black masterbatch at 1.5–3.0 wt%, resulting in 2.0–2.5% final carbon black when a 40% carbon black concentrate is used. The applicable specification is GRI-GM17 for linear low density polyethylene geomembranes; tests include ASTM D6693 for tensile properties, ASTM D5397 for stress crack resistance, and ASTM D1693 for ESCR. Terminal products are canal liners, landfill caps, temporary pond liners, and heap leach pad liners.
The critical process conflict is carbon black dispersion versus thermo-oxidative degradation. Carbon black masterbatch is side-fed or melt-dispersed before the flat die; agglomerates above 20 µm can initiate localized stress cracking at notched regions under service load. Residence time is limited to 3–5 min, and melt temperatures above 230°C reduce stress-crack resistance below the value required by ASTM D5397. Dimensional stability of the sheet is monitored by ASTM D5199 because thickness variation beyond ±5% creates thinning at the roll-down edge during field deployment. Post-extrusion cooling is controlled by a multi-roll calender stack to maintain flatness.
Drum liners at thicknesses of 100–250 µm are produced by blown film from DFDA-7510 NT at 65–85 wt%, LDPE at 10–20 wt%, slip masterbatch at 0.5–1.5 wt%, and colorant where required at 2–5 wt%; the formulation preserves Faraday fusion heat sealing, which is standard for circular drum liners. Compliance for chemical drum liners is anchored to REACH Regulation (EC) No 1907/2006 for EU article obligations and, for food-contact liners, 21 CFR 177.1520 and Regulation (EU) No 10/2011; the supplier certificate of analysis is needed when the liner will contact corrosive or oxidizing media. Process control on a 50–75 mm extruder with L/D 25:1–30:1, die gap 1.5–2.5 mm, and blow-up ratio 2.0:1–2.8:1 holds pinhole frequency below one pinhole per 10 m². Terminal products include aseptic culture liners, solvent drum liners, powder chemical liners, and waste disposal drum liners.
Extrusion coating a 15–35 g/m² layer of DFDA-7510 NT onto kraft paper requires die melt temperatures of 300–330°C, but resin residence time at that temperature should not exceed 6–8 min because thermo-oxidative chain scission reduces adhesion and increases gel formation. The formulation is 90–100 wt% DFDA-7510 NT with LDPE at 0–10 wt% for draw stability; slip and antiblock are omitted because they impair paper adhesion. Compliance for food-contact multiwall sacks includes 21 CFR 177.1520 for the polyethylene layer and 21 CFR 176.170 for the paper component, plus Regulation (EU) No 10/2011 with overall migration ≤10 mg/dm² by EN 1186. The production line uses a 90–120 mm extruder with L/D 26:1–30:1, automated die lip gap of 0.4–0.8 mm, chill roll temperature 10–20°C, and nip pressure 150–300 N/cm to force the melt into paper fiber interstices. Terminal products include multiwall paper sacks, aluminum-free desiccant bag laminates, and industrial paper wrap. Edge bead thickness is kept within ±10% of center coating weight, and melt curtain neck-in is controlled below 15% by die-to-chill-roll spacing adjustments.
Competitive Dow FINGERPRINT™ DFDA-7510 NT Linear Low Density Polyethylene Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Dow FINGERPRINT™ DFDA-7510 NT is an ethylene-butene linear low density polyethylene resin supplied in pellet form for blown film extrusion and selected cast film and sealant-web applications. Supplier-published base-resin parameters place the melt mass-flow rate at 1.0 g/10 min measured at 190 °C under 2.16 kg load according to ASTM D1238 or ISO 1133-1, and the density at 0.920 g/cm³ determined by ASTM D792 or ISO 1183-1. The NT suffix denotes a natural resin supplied without an intentionally added slip agent or antiblock package; the converter introduces slip and antiblock masterbatches to adjust the coefficient of friction of the finished film. The grade is positioned for monolayer and coextruded packaging structures in which the film must balance tensile strength, puncture resistance, and optical clarity. Because the polymer backbone is linear and the short-chain branching distribution is controlled by the polymerization system, the melt rheology differs from high-pressure low density polyethylene of equivalent density and melt index, and that difference governs both the processing window and the end-use property set.
On blown film lines using single-screw extruders with 24:1 to 30:1 L/D ratios, the melt temperature should be maintained in the 190 °C to 230 °C range. Melt temperatures above 240 °C increase the risk of oxidative gel formation and visible film specks, particularly when screen packs are partially blinded or when residence time is extended by a long adaptor. A typical barrel profile is flat-to-rising: feed zone 170 °C to 180 °C, compression zone 190 °C to 210 °C, metering zone 210 °C to 225 °C, and die at 220 °C to 230 °C. The die gap should be set at 1.8 mm to 2.5 mm; this reduces interfacial melt fracture compared with the 0.8 mm to 1.0 mm gaps commonly used for high-pressure low density polyethylene. Because DFDA-7510 NT has lower melt strength and stronger extension-thinning behavior than high-pressure LDPE of the same melt index, the blow-up ratio is typically restricted to 2.0 to 3.0, and the frost line height is set at 6 to 10 die diameters to preserve a stable bubble geometry. Output on a 60 mm grooved-feed extruder fitted with a 200 mm die is usually constrained by melt pressure rather than screw torque; screen pack and breaker plate pressure drop should therefore be monitored, and the screen pack should be changed when the pressure exceeds the extruder manufacturer’s alarm setting. Process conditions for a given line may require a polymer processing aid, typically at 200 ppm to 800 ppm by weight, to control die lip buildup and sharkskin melt fracture. Pre-drying is not normally required for sealed, dry pellets, but material stored in unheated warehouses with repeated cold-to-warm cycling at relative humidity above 60 % should be dried for at least 2 h at 80 °C to avoid surface moisture and bubble pinholes. Films blown from DFDA-7510 NT at a nominal gauge of 25 µm exhibit haze and dart impact responses that depend on frost line height, die gap, and the amount of high-pressure LDPE added; published data for this specific line configuration is limited, and converter-scale verification on the target line is required.
Supplier-published base-resin values are reproduced below to support incoming resin quality verification. A density or melt-flow deviation greater than the supplier’s accepted lot tolerance should trigger a rheological check and a purge before film production starts.
| Parameter | Test method | Published value |
|---|---|---|
| Melt mass-flow rate at 190 °C, 2.16 kg | ASTM D1238 / ISO 1133-1 | 1.0 g/10 min |
| Density | ASTM D792 / ISO 1183-1 | 0.920 g/cm³ |
| Form | Visual inspection | Pellets |
| Additive package | Supplier information | Natural resin; no slip or antiblock added |
Regulatory status for food-contact use is determined by the finished article and its conditions of use, not by the bulk resin alone. The base resin is typically evaluated under the olefin polymer provisions of FDA 21 CFR 177.1520(c) and, for European Union food-contact packaging, under Regulation (EU) No 10/2011 with an overall migration limit of 10 mg/dm². Compliance must be confirmed by migration testing on the finished package because additive masterbatches, printing inks, coatings, and lamination solvents change the final food-contact profile. REACH registration requirements under Regulation (EC) No 1907/2006 apply to the supplier; converters should request a supplier SVHC declaration and a statement under Directive 2011/65/EU where packaging components enter electrical and electronic product streams.
Relative to a high-pressure LDPE having the same 0.920 g/cm³ density and 1.0 g/10 min melt index, DFDA-7510 NT has a linear molecular architecture without long-chain branching. The practical consequence is lower zero-shear viscosity, less shear thinning, and lower melt strength. On the same blown film die with a narrow 0.8 mm gap, LLDPE grades in this density and melt index class frequently show sharkskin melt fracture, whereas high-pressure LDPE processes without visible surface disruption. Compared with high-pressure LDPE, DFDA-7510 NT normally provides higher tensile strength, dart impact, and puncture resistance at equal film gauge, but the bubble is less forgiving of air-ring fluctuation, and the melt response may produce lower machine-direction tear strength in some formulations. Against a metallocene-catalyzed LLDPE of similar density and melt index, DFDA-7510 NT generally has a broader molecular weight distribution, which improves torque stability and melt-pressure control on older extruders but may produce a higher gel count and slightly higher haze. The FINGERPRINT™ designation within the Dow polyethylene portfolio is associated with optical consistency and reduced visual defects; however, such claims should be evaluated by film haze measurement according to ASTM D1003, gel count via a quantitative visual gel-count method, and coefficient of friction by ISO 8295 or ASTM D1894 after the selected slip or antiblock masterbatch has been compounded. Against other butene-copolymer LLDPE grades of the same density and melt index, DFDA-7510 NT is specified by the supplier for applications requiring improved clarity and lower speck level, but published data for exact comparative values is limited and must be verified on the target line. The molecular weight distribution and comonomer distribution should be compared by GPC, DSC, or dynamic rheological testing when the grade is considered as a drop-in replacement for another butene LLDPE.
In three-layer and five-layer coextruded films, DFDA-7510 NT is commonly assigned to the sealant layer because its sealing initiation temperature is lower than high-density polyethylene and its hot-tack strength is sufficient for vertical form-fill-seal packaging. Seal initiation is measured by ASTM F1921 or JIS Z 1707; hot tack is measured by ASTM F1921 Method B or a hot-tack rig at dwell times of 0.5 s and seal pressure of 0.3 MPa. For linear low density polyethylene resins in this density and melt-flow class, seal initiation typically falls between 95 °C and 105 °C, but the exact value for DFDA-7510 NT should be confirmed by laboratory heat-seal testing because coextrudate skin-layer thickness, cooling rate, and additive migration shift the hot-tack envelope. When a coextruded sealant layer is run at a thickness below 15 µm, melt-film stability can deteriorate; increasing the sealant-layer melt temperature to the upper end of the recommended range and reducing die-lip air velocity are common corrective actions. Corona treatment of the sealant layer for lamination should target a wetting tension of 38 mN/m to 46 mN/m after treatment, but the watt density and electrode configuration are line-specific.
In collation shrink and laminate film structures, DFDA-7510 NT is often blended with 10 wt% to 20 wt% high-pressure LDPE to increase bubble stability and improve optical smoothing without fully sacrificing LLDPE toughness. Published processing experience indicates that a 15 wt% LDPE addition widens the bubble-stability window by raising melt strength and lowering die pressure; however, the exact optimum depends on the extruder screw design, die diameter, and film gauge. Shrink response is measured by ISO 14616 or ASTM D2732 on samples cut in the machine and transverse directions after exposure to controlled hot air. LLDPE-rich films generally show lower free shrink than LDPE-rich films at a given temperature but higher shrink force and puncture resistance. The film’s tensile properties should be tested by ASTM D882 or ISO 527-3, dart impact by ASTM D1709 Method A or Method B, and tear by ASTM D1922 or ISO 6383-2. When a laminate film is pouch-sealed, the sealant layer prepared from DFDA-7510 NT should be heat-seal tested after corona treatment because surface energy decay and additive bloom can reduce seal strength. The blend ratio should be controlled gravimetrically; batch-to-batch scatter in melt index and density within the supplier’s specification can shift the frost line height and seal initiation temperature, so incoming lot data should be recorded against the supplier certificate of analysis for each production run.
Quality verification begins with the supplier certificate of analysis listing melt flow rate and density. Incoming resin should be sampled and tested for bulk density, pellet contamination, and foreign material. Film samples should be collected only after the line reaches steady-state, at least 30 min after any setpoint change. Haze is measured according to ASTM D1003, clarity via ASTM D1746 or a wide-angle hazemeter, gloss at 45° by ASTM D2457, and coefficient of friction by ISO 8295 after 24 h conditioning at 23 °C and 50 % RH. Because the NT grade contains no slip or antiblock, the measured film coefficient of friction will be high unless a masterbatch is added; typical slip levels are 500 ppm to 1,000 ppm erucamide and 2,000 ppm to 5,000 ppm silica or synthetic silica antiblock, but the exact addition should be determined by the converter’s coefficient-of-friction target and food-contact status. Additive migration kinetics in polyolefin matrices are slow; coefficient of friction may continue to decline over 24 h to 72 h after film production, so packaging line trials should not be conducted immediately after winding. Storage of film rolls in a controlled environment at 15 °C to 25 °C and 40 % RH to 60 % RH reduces blocking and surface haze drift. The resin should not be combined with amine-based additives that can promote yellowing or with nitrosating agents; if purging a previous resin, a linear-low-density polyethylene or dedicated purging compound should be used, and the line should be purged until melt pressure and melt temperature return to the prescribed setpoints for DFDA-7510 NT.