| HS Code | 827746 |
| Density | 0.923 g/cm³ |
| Meltindex | 0.85 g/10 min |
| Meltflowratio | 8.5 (I10/I2) |
| Meltingpoint | 123 °C |
| Vicatsofteningpoint | 103 °C |
| Tensilestrengthatbreak | 32 MPa |
| Elongationatbreak | 700% |
| 1 Secantmodulusmd | 200 MPa |
| 1 Secantmodulustd | 220 MPa |
| Dartdropimpact | 200 g |
| Elmendorftearmd | 220 g |
| Elmendorfteartd | 440 g |
| Haze | 6% |
| Gloss | 70 (45°) |
| Coefficientoffriction | 0.2 |
As an accredited Dow ELITE™ 5230G Enhanced Polyethylene Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Dow ELITE™ 5230G Enhanced Polyethylene Resin is packaged in 25 kg moisture-resistant, polyethylene-lined bags, palletized for convenient handling and storage. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): Dow ELITE™ 5230G in 25 kg bags, 1,000 bags, 25 MT net, floor-loaded and securely stowed. |
| Shipping | Dow ELITE 5230G Enhanced Polyethylene Resin ships as non-hazardous solid pellets in 25 kg bags, bulk bags, or bulk trucks/railcars. Keep containers closed, dry, and out of direct sunlight. Avoid excessive heat and ignition sources. Not classified as dangerous goods for transport; handle per local regulations. |
| Storage | Store Dow ELITE™ 5230G Enhanced Polyethylene Resin in a cool, dry, well-ventilated area away from direct sunlight, heat, flames, and strong oxidizers. Keep containers or bags closed to prevent moisture, dust, and contamination. Avoid prolonged UV exposure and extreme temperatures. Use first-in, first-out stock rotation. Stack pallets securely and follow local regulations and the supplier’s safety data sheet. |
| Shelf Life | Shelf life is 24 months from date of manufacture when stored in unopened original packaging at temperatures below 50°C, protected from direct sunlight. |
In frozen-food vertical form-fill-seal (VFFS) packaging lines operating at 80–120 packages/min, the sealant web is subjected to cold-rupture forces at −25 °C and jaw-face compression at 90–120 °C within the same cycle. Dow ELITE™ 5230G Enhanced Polyethylene Resin is formulated at 70–85 wt% with 15–30 wt% high-pressure LDPE having a melt index of 0.25–0.75 g/10 min to stabilize the bubble on a three-layer blown-film die while retaining a seal initiation window of 95–105 °C under ASTM F2029 heat-seal gradient testing. The regulatory boundary for food-contact use rests on FDA 21 CFR 177.1520(c) 3.1a and 3.2a, EU Commission Regulation (EU) No 10/2011 Annex I, and China GB 4806.6-2016; total migration is tested under EN 1186-1:2002 with aqueous, acidic, and olive oil simulants, while moisture vapour transmission is quantified under ASTM F1249. The downstream process on a 90 mm single-screw extruder with L/D 30:1 and a barrier screw uses a 60/80/100 mesh screen pack, delivering melt at 200–215 °C to a 350 mm die with a die gap of 2.0–2.4 mm; the blow-up ratio is maintained at 2.2:1–2.8:1 and frost-line height at 600–900 mm to control MD/TD tear balance. Corona treatment is applied at 36–38 mN/m per ASTM D2578 before gusseting. The resulting 40–80 µm film is converted into pillow pouches for individually quick-frozen vegetables, frozen seafood bags, and freezer overwrap for bakery products.
Limitations observed on production lines include crease-leaker formation when the film reaches the sealing jaws with surface frost from cold storage; this is a condensation boundary rather than resin moisture because the polymer is non-hygroscopic. Gauge variation across the layflat must be held below ±5% because the VFFS film tracks over forming collars under tension. Antiblock masterbatch is added only in the outer skin layer at 1–3 wt% if blocking occurs; addition above this threshold measurably raises haze under ASTM D1003 and reduces hot tack under ASTM F1921. The food-contact grade must be tested in the finished laminate, not only on the pellet, because sealing aids and corona treatment alter the surface contact layer.
| Application | Standard / clause | Parameter controlled |
|---|---|---|
| Frozen-food VFFS films | FDA 21 CFR 177.1520(c) 3.1a / 3.2a | Olefin polymer base resin compliance |
| Frozen-food VFFS films | EU 10/2011 Annex I | Overall migration ≤ 10 mg/dm² |
| Heavy-duty industrial liners | ASTM D1709, ASTM D1922, ASTM D5748, ISO 527-3 | Dart impact, Elmendorf tear, puncture, tensile |
| Stretch hood pallet film | ASTM D5458, ASTM D5748, ISO 527-3 | Cling force, puncture resistance, tensile modulus |
| High-barrier pouch sealant web | FDA 21 CFR 177.1520(c) 3.1a, EU 10/2011, GB 9685-2016 | Sealant layer compliance and additive migration |
| Agricultural silage / greenhouse film | EN 13206:2017, ISO 4892-2:2013 | Weathering, retained elongation, UV degradation |
The extrusion of heavy-duty industrial liners on high-stalk blown-film towers with internal bubble cooling (IBC) exposes the melt to extensional stress at the die exit and long residence time in the tower; bubble flutter typically increases when the frost-line height is raised without a corresponding increase in low-shear melt strength. In this structure, ELITE 5230G is loaded at 55–75 wt% with 20–30 wt% post-industrial recycled LLDPE/HDPE regrind and 3–8 wt% carbon black masterbatch with active carbon content of 40–50%. The function of the regrind fraction is not dilution but rheological stiffening; a regrind fraction above 30 wt% produces melt-pressure fluctuations across the screen pack and visible blue-grey specks at the die lip. Compliance for heavy-duty industrial film is performance-based rather than food-contact-based; tear resistance is quantified under ASTM D1922, dart impact under ASTM D1709, slow puncture under ASTM D5748, and tensile properties under ISO 527-3. When the liner is used as an inner packaging for dangerous goods, the combined package is type-approved under the applicable UN dangerous goods packaging code, not the resin itself; the drop-test requirement under 49 CFR 178.603 is applied at the sack level. The terminal articles are 100–200 µm construction aggregate sacks, mineral-filler liners, and chemical-powder liners.
Processing on a 120 mm extruder with L/D 30:1 and IBC uses a die gap of 2.2–2.5 mm, a blow-up ratio of 1.8:1–2.5:1, and melt temperatures from 210–235 °C. Frost-line height is usually set between 900–1400 mm; when the frost line is lowered below this window to raise output, transverse direction tear drops because the film is drawn more rapidly in the machine direction. Carbon black agglomerates at the die lip are a common field failure; the screen pack is staged at 60/80/100 mesh and the die gap is inspected at shift changes. Published data for this specific blend configuration is limited, so starting ratios should be adjusted only after measuring dart impact and tear retention on the finished film. Film property inconsistency from post-industrial regrind is controlled by sieve analysis and melt-filter pressure monitoring rather than by accepting bulk resin certification alone.
Pallet unitization stretch hood lines impose a different stress state than standard collation shrink film because the film tube is mechanically opened and drawn over a 1,000 mm × 1,200 mm pallet at high speed, requiring elastic recovery at the top corners and puncture resistance at contact points with sharp package edges. In this application, ELITE 5230G is loaded at 75–90 wt% with 10–25 wt% high-pressure LDPE or fractional-melt LLDPE to balance cling force against puncture resistance; the film is typically 120–180 µm thick. ASTM D5458 cling force, ASTM D5748 puncture resistance, and ISO 527-3 tensile modulus are the controlling test methods. Production is carried out on a high-stalk blown-film line with 2.5 mm die gap and blow-up ratio of 2.8:1–3.5:1; melt temperature is held at 210–225 °C, and internal bubble cooling is required to prevent bubble flutter at the high blow-up ratio. Adding LDPE above 25 wt% raises peel cling but measurably lowers puncture resistance; below 10 wt%, bubble stability on the high-stalk tower becomes the limiting factor. Anti-block is used sparingly at 2,000–4,000 ppm active synthetic silica because excessive anti-block lowers cling force and increases haze under ASTM D1003. The terminal product is a pallet hood for bagged construction materials, white goods, and ceramic tiles.
Failure modes observed on production lines include corner thinning when the film tube is opened off-centre and edge fold cracks when the frost line is too low. The film is driven by elastic recovery rather than shrink energy, so the stretch hood requires a non-blocking surface. Film gauge is verified under ASTM D5940 on the collapsed layflat, not only at the die, because edge folds can be masked by web tension. The LDPE co-blend fraction must be monitored for gel content under ASTM D2765 if recycled LDPE is introduced, since gel particles can localise stress at the corner stretch zone during dynamic pallet loading.
| Application | ELITE 5230G loading (wt%) | Co-blend / masterbatch | Film thickness |
|---|---|---|---|
| Frozen-food VFFS film | 70–85 | 15–30 wt% LDPE, 1–3 wt% antiblock skin | 40–80 µm |
| Heavy-duty industrial liner | 55–75 | 20–30 wt% recycled LLDPE/HDPE, 3–8 wt% carbon black masterbatch | 100–200 µm |
| Stretch hood pallet film | 75–90 | 10–25 wt% LDPE or fractional-melt LLDPE, 2,000–4,000 ppm synthetic silica | 120–180 µm |
| High-barrier pouch sealant web | 85–95 | 5–15 wt% antiblock masterbatch, 2–5 wt% slip masterbatch | 20–35 µm |
| Agricultural silage / greenhouse film | 82–92 | 8–18 wt% carbon black/UV or 1–3 wt% HALS/UV plus 2–5 wt% anti-fog | 25–50 µm silage, 150–200 µm greenhouse |
High-barrier pouch structures for dry powders and frozen foods require a sealant web that can be sealed through a lamination layer at high speed without thermally stressing the barrier substrate. The sealant web is processed as a blown film at 20–35 µm and laminated to 12 µm metallized polyester or 20 µm biaxially oriented polypropylene by solventless adhesive. ELITE 5230G is used at 85–95 wt% with 5–15 wt% anti-block masterbatch having synthetic silica active content of 10–20%, and 2–5 wt% slip masterbatch with erucamide active content of 5%. The slip and antiblock package is split between the skin layers to prevent bloom-driven seal contamination. Food-contact compliance is tied to FDA 21 CFR 177.1520(c) 3.1a, EU 10/2011 Annex I, and GB 9685-2016 for additives; heat-seal strength is measured under ASTM F88/F88M and hot-tack under ASTM F1921. Blown-film processing uses a die gap of 1.8–2.2 mm, blow-up ratio of 2.0:1–2.5:1, and melt temperature of 190–210 °C; the film is corona-treated to 38–40 mN/m for acceptable lamination bond strength. The terminal articles are stand-up pouches for dried dairy powders, snack foods, and frozen fruit. Published data for the specific seal initiation temperature of this configuration is limited; the actual window should be determined by heat-seal gradient testing under ASTM F2029.
The lamination adhesive, not the resin, often dictates shelf-life under high humidity. The PE sealant remains non-hygroscopic, but surface condensation on the corona-treated film can reduce adhesive wetting. The sealant web is not suitable for retort or pasteurisation above 100 °C because seal strength and dimensional stability decline; uses must remain below boiling point. Avoid excessive silicone slip additive because it lowers lamination bond strength and can produce delamination at the pouch gusset fold. When the coextruded slip layer is placed on both outer surfaces, the coefficient of friction under ASTM D1894 must be maintained above 0.25 to prevent the film from tracking on the packaging machine forming collar.
Agricultural silage wrap is exposed to UV radiation, organic acids from fermented forage, and cyclic elongation during bale wrapping. In this scenario, ELITE 5230G is compounded at 82–92 wt% with 8–18 wt% carbon black/UV masterbatch for black silage film; transparent greenhouse covering uses 1–3 wt% HALS/UV stabilizer masterbatch and 2–5 wt% anti-fog additive package. The three-layer coextrusion line uses die gap 2.2 mm, blow-up ratio 2.3:1–2.8:1, and melt temperature 200–220 °C; silage wrap is calendered to 25–50 µm, while greenhouse cladding is run at 150–200 µm. Compliance for greenhouse films is governed by EN 13206:2017, and accelerated weathering is validated under ISO 4892-2:2013 with xenon-arc exposure; retained elongation at break is the critical endpoint. The terminal products are round bale silage wrap and tunnel greenhouse covers. Failure at the bale wrapper originates at acid-etched film surfaces where silage leachate has reduced tear resistance; therefore the carbon black masterbatch must be dispersed through a 40–50% active carbon black and screened at 80/100 mesh to avoid microvoids.
Published data for specific UV additive retention in ELITE 5230G is limited; formulators should verify stabilizer migration and extraction by ISO 4892-2 and Fourier-transform infrared spectroscopy after accelerated weathering. Processing boundaries are defined by the greenhouse cover film drawing ratio; when the film is thinned below 150 µm for tunnel cladding, multi-season tear retention becomes the limiting factor rather than the resin’s initial mechanical properties. Black silage film must be wound under controlled tension because the carbon black masterbatch increases surface roughness and can shift the coefficient of friction under ASTM D1894 beyond the bale wrapper’s feed tolerance.
Competitive Dow ELITE™ 5230G Enhanced Polyethylene Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Dow ELITE™ 5230G Enhanced Polyethylene Resin is an ethylene-octene copolymer supplied in pellet form for blown film extrusion and coextrusion. The grade is produced by a solution polymerization process using a constrained-geometry catalyst system that yields a narrow molecular weight distribution and controlled comonomer placement. Nominal density is 0.916 g/cm³ under ASTM D792, and nominal melt index is 4.0 g/10 min under ASTM D1238 at 190°C with a 2.16 kg load. These values place the resin in the low-density polyethylene range while retaining linear low-density polyethylene short-chain branching architecture. The octene comonomer contributes ethyl branches to the polyethylene backbone, and the narrow composition distribution reduces the formation of large, isolated crystalline domains that scatter light and initiate brittle fracture. The resin is therefore specified where downgauging, optical clarity, and seal integrity must be maintained simultaneously. The product is not a long-chain-branched autoclave LDPE; bubble stability and melt strength follow LLDPE rheology rather than high-pressure LDPE rheology.
The molecular weight distribution of 5230G is narrower than that of conventional butene LLDPE of equivalent melt index, and the comonomer is incorporated more uniformly across the chain-length distribution. This architecture shifts the solid-state deformation mechanism from low-stress craze propagation to shear yielding, which is measured as higher Elmendorf tear and dart impact at constant gauge. The rheological consequence is a reduced low-shear viscosity at equivalent melt index but more pronounced shear-thinning behavior in the apparent viscosity-shear rate curve, allowing increased extruder throughput without a proportional increase in melt temperature. Comparative evaluations on a 45 mm barrier screw with 24:1 L/D at 40 kg/h typically show lower die pressure for 5230G than for a butene LLDPE of 4.0 g/10 min melt index. The absence of long-chain branching does not provide LDPE-like melt strength; bubble stability is therefore more dependent on internal bubble cooling and air ring selection than is the case with high-pressure LDPE. Capillary rheometry data should be obtained from the supplier for lot-specific shear viscosity values, because published data for this specific configuration is limited.
On production-scale blown film lines, the resin is processed at melt temperatures between 190°C and 220°C. A typical barrel profile from feed throat to die is 170/180/190/200/210/215°C on a 75 mm grooved-feed extruder with a 30:1 L/D barrier screw and a 250 mm spiral mandrel die with a 1.2 mm die gap. Bubble stability is maintained at blow-up ratios from 2.0:1 to 3.0:1, and frost line heights of 600 mm to 900 mm are typical with internal bubble cooling. Output is usually limited by cooling capacity rather than melt fracture, because the onset of sharkskin is shifted to higher shear rates compared with butene LLDPE of the same melt index. Surface defects at the die lip can be reduced by using a die gap of at least 1.0 mm and by maintaining die temperature within 5°C of the adapter temperature. A barrier screw with compression ratio between 2.2:1 and 3.0:1 and a Maddock mixing section improves colorant dispersion and reduces melt temperature variation. The resin is compatible with conventional LLDPE screw geometries; a metering depth of 3.5 mm to 4.5 mm on a 75 mm screw is adequate to avoid excessive melt residence time.
The following table lists nominal physical properties reported for 25 µm monolayer blown film and for the pellet. Values are not lot specifications; the supplier certificate of analysis should be used for production acceptance.
| Property | Test method | Nominal value |
|---|---|---|
| Melt index | ASTM D1238 | 4.0 g/10 min |
| Density | ASTM D792 | 0.916 g/cm³ |
| Vicat softening point | ASTM D1525 | 102°C |
| Melting point | ASTM D3418 | 122°C |
| Haze | ASTM D1003 | 8.0% |
| Gloss at 45° | ASTM D2457 | 75 |
| Dart impact F50 | ASTM D1709 Method A | 250 g |
| Elmendorf tear MD | ASTM D1922 | 300 g |
| Elmendorf tear TD | ASTM D1922 | 350 g |
| Tensile strength at break MD | ASTM D882 | 42 MPa |
| Tensile strength at break TD | ASTM D882 | 36 MPa |
| Elongation at break MD | ASTM D882 | 600% |
| Elongation at break TD | ASTM D882 | 700% |
Food packaging and heavy-duty shipping sack structures use 5230G in sealant webs and outer plies where puncture and tear resistance are critical. The resin can be coextruded with HDPE or EVOH without adhesion issues when a maleic anhydride-grafted tie resin is used in the adjacent layer. Seal strength of 12 N/15 mm is typically reached at seal bar temperatures between 115°C and 130°C on a dwell-time heat sealer at 0.5 s dwell and 0.3 MPa jaw pressure. The hot tack plateau is broad; cohesive failure remains the dominant failure mode up to 135°C. Haze values below 10% are achievable in monolayer structures at 25 µm, but coextrusion with HDPE skins may raise haze depending on layer ratio. The optical contribution of 5230G in a coextruded structure is limited by total film thickness and by the surface layer.
In coextruded sealant layers, substitution of 5230G for LDPE or butene LLDPE requires adjustment of frost line height and air ring pressure because the melt tension of 5230G is lower than that of LDPE. Blending 10–20 wt% high-pressure LDPE restores bubble stability without eliminating the optical and toughness advantages. Compared with butene LLDPE of equivalent density and melt index, 5230G exhibits higher Elmendorf tear and dart impact at the same gauge; the improvement is attributed to a higher tie-molecule population generated by the octene branches. The seal initiation temperature is typically 5–10°C lower than that of a butene LLDPE of identical melt index, which permits faster packaging line speeds and lower jaw temperature setpoints. Relative to lower-MI ELITE grades, 5230G provides higher extruder output but lower dart impact and tear; a fractional-MI grade may be required for frozen-food packaging where low-temperature puncture resistance dominates. Because 5230G lacks long-chain branching, it cannot be used as a direct substitute for LDPE in high-melt-strength applications such as foam extrusion or curtain coating without blending.
Below -20°C, the dart impact retention of 5230G is governed by the beta-relaxation of the ethylene-octene crystal phase and by the concentration of tie molecules. The resin has been evaluated in frozen-food packaging at film thicknesses from 25 µm to 75 µm; retained dart impact at -20°C is reported to be above 80% of ambient value in supplier technical literature, although published data for this specific configuration is limited. Low-temperature performance is superior to butene LLDPE of equivalent density but inferior to fractional-MI octene grades with higher molecular weight. The selection of 4.0 g/10 min melt index represents a compromise between low-temperature toughness and line throughput; processors running frozen-food structures at high output typically select a 1.0 g/10 min grade for the core layer and retain 5230G in the sealant layer.
Production-scale experience indicates that screw design influences gel formation and output stability. Barrier screws with compression ratios between 2.2:1 and 3.0:1 and screen packs of 40/80/120 mesh are used to homogenize the melt and trap crosslinked particles. Melt temperatures above 235°C are not recommended because oxidative degradation can increase gel counts and reduce film tear resistance. Purge with a fractional-MI LDPE between product transitions, and avoid direct transition from HDPE to 5230G without purging because viscosity mismatch can leave stagnant resin in the manifold. The resin is not hygroscopic, but surface condensation can occur after cold storage; pellets should be brought to ambient temperature in the original sealed packaging to avoid moisture on the film surface. Die lip fouling has been observed at high screw speeds when the frost line is set below 600 mm; increasing frost line height or reducing screw speed resolves the defect. Fluoropolymer processing aids at 200–500 ppm can reduce die lip fouling in long campaigns, but their use must be validated for food-contact compliance.
Food-contact compliance for 5230G is evaluated under the resin supplier regulatory documentation. The polyethylene base resin is manufactured to meet the compositional requirements of FDA 21 CFR 177.1520(c)(2.1) for olefin polymers intended for contact with food, subject to the conditions of use specified in 21 CFR 176.170(c). Compliance with EU Regulation (EU) No 10/2011, Annex I, Table 1 is reported by the supplier for overall migration below 10 mg/dm² under the test conditions of OM2 or OM3 depending on the intended food type. REACH registration under EC No 1907/2006 covers the monomer and polymer substances; the resin contains no substance of very high concern above 0.1 wt% per article. RoHS Directive 2011/65/EU, Annex II restrictions on lead, mercury, cadmium, hexavalent chromium, polybrominated biphenyls, and polybrominated diphenyl ethers apply to electrical and electronic equipment rather than packaging; however, the resin is typically certified as compliant with the maximum concentration values when tested by XRF screening.
| Regulation or standard | Scope | Status |
|---|---|---|
| FDA 21 CFR 177.1520(c)(2.1) | Olefin polymers for food contact | Supplier declaration |
| EU (EU) No 10/2011, Annex I, Table 1 | Plastic food contact materials | Overall migration 10 mg/dm² |
| REACH (EC) No 1907/2006, Annex XVII | Restrictions on hazardous substances | No SVHC above 0.1 wt% |
| RoHS Directive 2011/65/EU, Annex II | Restricted substances in EEE | Below MCV by XRF |
Final compliance of a converted article depends on additives, printing inks, coatings, and the specific food contact conditions; users must obtain the full regulatory data package from the supplier and evaluate the final package under the applicable migration test methods.