| HS Code | 310449 |
| Resintype | Enhanced Polyethylene |
| Density | 0.918 g/cm³ |
| Meltindex 190c 2 16kg | 0.85 g/10 min |
| Meltflowratio I21 I2 | 32 |
| Meltingpoint | 122 °C |
| Vicatsofteningpoint | 100 °C |
| Crystallizationtemperature | 104 °C |
| Dartdropimpact | 300 g |
| Elmendorftearstrength Md | 300 g |
| Elmendorftearstrength Td | 500 g |
| Tensilestrengthatyield Md | 1400 psi |
| Tensilestrengthatyield Td | 1400 psi |
| Tensilestrengthatbreak Md | 5000 psi |
| Tensilestrengthatbreak Td | 4500 psi |
| Elongationatbreak Md | 600% |
| Elongationatbreak Td | 700% |
| Secantmodulus 1pct Md | 26000 psi |
| Secantmodulus 1pct Td | 30000 psi |
| Haze | 9% |
| Gloss 45deg | 70 |
| Coefficientoffriction | 0.2 |
As an accredited Dow ELITE™ 5110G Enhanced Polyethylene Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Dow ELITE™ 5110G Enhanced Polyethylene Resin is supplied in 25 kg polyethylene-lined paper bags, 40 bags per pallet (1,000 kg). |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): Dow ELITE™ 5110G Enhanced Polyethylene Resin in palletized 25 kg bags, dry, secure stowage. |
| Shipping | Dow ELITE™ 5110G Enhanced Polyethylene Resin is shipped as non-hazardous, solid pellets in 25 kg bags, bulk bags, or bulk trucks/railcars, often palletized and stretch-wrapped. Keep containers closed; store cool and dry, away from sunlight, moisture, and ignition sources. Follow SDS and transport regulations. |
| Storage | Store Dow ELITE™ 5110G in a cool, dry, well-ventilated warehouse. Keep resin in original sealed bags on pallets, off the floor. Protect from moisture, direct sunlight, UV, excessive heat, flames, and contamination. Avoid strong oxidizers. Maintain clean, dry conditions, prevent dust buildup, use safe stacking limits, follow first-in, first-out stock rotation, and keep away from ignition sources and incompatible materials. |
| Shelf Life | Shelf life is typically 24 months from date of manufacture when stored in original packaging under cool, dry conditions. |
On a 75 mm single-screw extruder with a 30:1 L/D barrier screw and grooved feed zone, Dow ELITE™ 5110G Enhanced Polyethylene Resin is processed into 80–140 µm monolayer heavy-duty sack film. The screen-pack sequence 40/60/80 mesh is placed ahead of a 350 mm spiral mandrel die with a die gap of 1.8 mm, producing adapter melt pressures of 280–320 bar at melt temperatures of 210–230 °C. A blow-up ratio of 2.5:1 is held by a dual-lip air ring operating at 5.5 m³/min per metre of die circumference; frost line height is controlled at 3–4 die diameters above the air ring. Capacitance thickness scanning of the collapsed web shows gauge variation of ±5% at 220 kg/h output, rising to ±8% at 260 kg/h if the die gap is not opened to 2.0 mm. Tensile yield stress in machine direction, measured according to ASTM D882-18, typically falls within 8–14 MPa for 100 µm LLDPE films depending on draw ratio and quench rate; grade-specific values are confirmed against the certificate of analysis. Dart impact resistance measured by ASTM D1709-16a, Method B is strongly influenced by bubble cooling intensity and die gap; insufficient air-ring flow reduces transverse orientation and lowers puncture energy under ISO 7765-1:2004. Carbonyl index measured by FTIR increases after prolonged melt residence at temperatures above 230 °C; total residence time is therefore limited to 12 minutes and purge cycles are triggered when melt pressure exceeds 350 bar. Rheological evaluation by rotational rheometry at 190 °C and 0.1–100 rad/s shows shear-thinning behaviour; melt flow rate determined by ASTM D1238-20, Procedure A at 190 °C/2.16 kg is used for incoming lot control because it correlates with extruder backpressure in the grooved feed section. Barrel temperature profile from hopper to die is set at 180 °C/210 °C/220 °C/230 °C/230 °C; pressure below 180 bar indicates a higher-melt-flow lot and lower bubble stability, while pressure above 300 bar indicates insufficient preheat or gel accumulation. Batch-to-batch coefficient of friction determined by ASTM D1894-14 shifts by less than 0.10 when slip and anti-block masterbatch at 1.5 wt% is dosed through the side feeder at feed throat temperature 40 °C.
In coextruded barrier films, the sealant skin layer is usually 12–20 µm within a 60 µm total structure. A five-layer line with separate extruders for the skin and tie layers prevents intermixing that raises seal initiation temperature by carrying higher-melting nylon or high-density polyethylene into the sealant interface. Seal initiation temperature is measured according to ASTM F2029-16 at 0.5 s dwell time and 0.275 MPa jaw pressure; LLDPE sealant formulations based on ELITE 5110G generally exhibit a seal initiation temperature of 90–105 °C, but the presence of 10 wt% HDPE regrind raises the onset by 5–8 °C. Hot tack strength measured by ASTM F1921-20 at 120 °C remains above 2.0 N/15 mm when the sealant layer is not diluted by more than 20 wt% of high-viscosity metallocene plastomer; above that concentration, hot tack decreases while seal strength plateaus. Processing on a seven-layer blown-film die with 2.0 mm die gap and 25:1 L/D skin extruders maintains melt temperatures of 215–235 °C at the adapter. Bubble cooling with internal bubble stabilisation is required when the sealant layer exceeds 20% of total thickness; without IBC, gauge variation increases from ±4% to ±7% at 250 kg/h output. Seal strength after contamination with common packaging liquids is assessed under ASTM F88/F88M-21 as a go/no-go control; a minimum average seal strength of 12 N/15 mm is commonly specified for 60 µm coffee pouch films, but published data for this specific configuration is limited. Conditioning at 23 °C and 50% RH for at least 40 h per ASTM D4332-14 is required before seal testing. Sealant layer thickness below 10 µm produces frequent burn-through on high-speed vertical form-fill-seal machines operating above 80 packages/min; a minimum skin layer of 15 µm is therefore used for coffee pouches and liquid detergent sachets.
| Requirement | Standard/Method | Typical Control Range |
|---|---|---|
| Melt flow rate | ASTM D1238-20, Procedure A, 190 °C/2.16 kg | 0.5–2.0 g/10 min |
| Density | ISO 1183-1:2019, Method A | 0.918–0.925 g/cm³ |
| FDA food contact | 21 CFR 177.1520(c) | Conforms |
| EU food contact | EU 10/2011, Annex I | Conforms |
| REACH | 1907/2006, Annex XVII | Conforms |
Extrusion lamination with ELITE 5110G is run on a single-screw extruder with a 30:1 L/D barrier screw and a 150 mm slot die. Melt temperature at the die is held between 290 °C and 320 °C to reduce neck-in and promote oxidation for adhesion. At an air gap of 150 mm and line speed of 150 m/min, neck-in per side is typically 4–6 cm; widening the die gap from 1.0 mm to 1.5 mm increases neck-in by 1–2 cm but improves gauge uniformity of the 20–30 µm coating. Corona treatment of aluminium foil to a surface energy above 42 dyn/cm determined by ASTM D2578-09(2017) is required; without primer, adhesion measured as T-peel strength per ASTM D1876-08(2015) remains below 4 N/15 mm, whereas an imine primer or ozone treatment raises peel strength above 8 N/15 mm. Melt draw resonance is observed when line speed exceeds 180 m/min at melt temperatures below 290 °C; draw resonance appears as periodic thickness variation with a wavelength of 10–15 mm. Raising the melt temperature to 310 °C and reducing the air gap to 100 mm suppresses the instability but reduces adhesion to paperboard unless corona intensity is increased to 45 dyn/cm. Kraft paper moisture content above 8 wt% reduces adhesion due to steam formation at the nip; preheating at 80 °C for 2 h reduces moisture to approximately 5 wt%. Melt pressure before the screen pack is maintained at 200–260 bar with a 60/80/100 mesh pack. Moisture vapour transmission rate of the finished laminate is tested according to ASTM F1249-20. High melt temperature above 320 °C produces free radical chain scission and visible gel particles after 10 minutes residence; die lip build-up increases from 0.5 g/h to 1.5 g/h and appears as coating streaks.
Stretch hood film of 80–120 µm gauge is extruded on a cast line equipped with a 75 mm, 25:1 L/D extruder and a 1.2 mm die gap. Melt temperature at the die is set at 230 °C and chill roll temperature is maintained at 20–25 °C to suppress post-crystallisation. Draw ratio between die exit and chill roll is kept below 12:1; above this ratio, Elmendorf tear strength measured by ASTM D1922-15 drops below 200 g in transverse direction for 100 µm film. Puncture resistance evaluated by ASTM D5748-18 is controlled by the base resin density and the absence of high-viscosity regrind; the addition of more than 15 wt% post-industrial stretch hood regrind increases gel specks above 0.5 mm² and lowers puncture energy by 10–15%.
Three-layer greenhouse film of 150–200 µm thickness is produced on a 1200 mm blown-film die with a 3.0:1 blow-up ratio. LLDPE resin provides the load-bearing layer between two UV-stabilised outer layers. Accelerated weathering under ASTM G154-16 Cycle 1 for 2000 h reduces tensile elongation at break measured by ISO 527-3:2018 to below 50% of initial value when the total hindered amine stabiliser concentration is below 0.4 wt%; increasing the stabiliser package to 0.6 wt% and including a phenolic antioxidant at 0.1 wt% retains elongation above 60% of initial after 2000 h. The resin layer is not pre-dried; condensation on pellets at relative humidity above 85% requires dry air purging at 70 °C for 2 h to prevent lens-shaped gel defects in the film. Pesticide resistance is assessed by immersion in sulphur-containing agrochemical solutions at 40 °C for 48 h; published data for this specific configuration is limited.
Competitive Dow ELITE™ 5110G Enhanced Polyethylene Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Dow ELITE™ 5110G Enhanced Polyethylene Resin is an ethylene/1-octene copolymer produced by a solution polymerization process and supplied in pellet form. The resin is classified as a linear low-density polyethylene with a nominal density of 0.9255 g/cm³ when determined according to ASTM D792 and a nominal melt index of 0.85 g/10 min when measured at 190 °C with a 2.16 kg load according to ASTM D1238. The enhanced designation derives from the single-site catalyst system and controlled polymer architecture rather than from post-reactor modification. This architecture produces a narrower comonomer distribution than conventional Ziegler-Natta LLDPE and a controlled population of long-chain branches that modifies melt elasticity.
The molecular weight distribution is proprietary, but rheological measurements show a shear-thinning response that is broader than a narrow molecular weight metallocene polyethylene and more controlled than a high-load-melt-index Ziegler-Natta resin. In blown-film conversion, this combination of shear thinning and extensional hardening supports bubble stability at higher blow-up ratios and increases output consistency on air-cooled external annular dies. Production-scale experience indicates that the resin transfers onto existing LLDPE lines without requiring screw changes when the extruder has an L/D ratio between 24:1 and 30:1. However, changes in melt pressure response and bubble cooling profile must be expected when moving from a broad-comonomer Ziegler-Natta resin; failure to rebalance the air ring after product change is a common cause of gauge variation and poor roll geometry.
| Nominal property | Value | Test basis |
|---|---|---|
| Density | 0.9255 g/cm³ | ASTM D792 |
| Melt index at 190 °C, 2.16 kg | 0.85 g/10 min | ASTM D1238 |
| Comonomer | 1-octene | Manufacturer designation |
| Physical form | Pellets | Manufacturer packaging specification |
The density value places the material in the lower-density region of the LLDPE family. This density reduces the crystalline fraction relative to a 0.935 g/cm³ medium-density polyethylene, lowering the seal initiation temperature and increasing low-temperature flexibility. The melt index of 0.85 g/10 min indicates a molecular weight high enough for blown-film toughness, yet low enough for stable extrusion through conventional film dies. A significant part of the product’s industrial utility is the combination of this density and melt index with 1-octene comonomer. Compared with a butene-based LLDPE of equal density and melt index, an octene-based copolymer can provide a higher proportion of tie molecules connecting crystalline lamellae after film stretching; this contributes to dart impact retention when film is downgauged. The exact molecular weight distribution and branch content are not disclosed in published data sheets, but the melt rheology shows a controlled degree of long-chain branching that is not typical of all single-site resins.
Barrel temperature profiles for a smooth-bore single-screw extruder are generally set from 170 °C in the feed zone to 210–230 °C in the metering and adapter zones. The melt temperature measured at the die entrance is maintained between 195 °C and 235 °C. The upper boundary is more critical than the lower one: at melt temperatures above 240 °C, residence-time-dependent thermal degradation can form oxidized gel particles, and film odour may increase. In high-output operations where screw speed is high, melt temperature should be monitored with an immersion thermocouple rather than inferred from barrel set-points.
Die gap and blow-up ratio interact. Industry practice for LLDPE film in this density class uses a die gap between 1.2 and 2.5 mm. For film above 80 µm, the upper end of this range reduces head pressure and melt fracture risk. For gauges below 30 µm, a thinner die gap increases draw and orientation, but the bubble can become more sensitive to air currents. Blow-up ratio is typically held between 2.0:1 and 3.5:1. Lower ratios improve gauge uniformity but reduce transverse direction tear resistance; higher ratios improve transverse properties but increase bubble wander and edge instabilities.
Frost-line height is set by the balance of extruder output, melt temperature, and air-ring flow. On a 75 mm extruder fitted with a 250 mm die and a dual-lip air ring, frost-line heights between 0.6 and 1.0 m above the die are common. A frost line that is too low produces a quenched skin with high haze and can increase blocking; a frost line that is too high permits the molten web to flow downward and creates gauge bands near the collapsing frame. Internal bubble cooling is often used above 150 kg/h output to remove heat from the inner bubble surface. Field data from air-cooled towers show that maximum stable output is frequently limited by cooling capacity rather than extruder torque.
Surface moisture is the main conditioning issue, not bulk moisture. If cold pellets are charged into a warm feed hopper, condensation can introduce bubbles into the melt. Pellets should be allowed to reach at least 5 °C above the plant dew point before hopper loading. Silos and surge bins should be purged with dry air when the resin is stored in high-humidity warehouses. The resin is not recommended for melt temperatures above 240 °C for long residence times; converters producing thin films at high output should optimize screw design to minimize stagnation points.
In heavy-duty sack and flexible intermediate bulk container applications, the product is used in monolayer films and coextruded structures where a balance of dart impact, tear resistance, and seal performance is required. Heavy-duty sack specifications frequently call for a dart impact value between 150 and 250 g on a 25 µm film tested according to ASTM D1709 Method A. These specifications are film-dependent; the same resin can produce different values when blow-up ratio, frost-line height, and die gap are changed. Converters should validate the product on the intended line rather than rely on a universal film property table.
Seal performance is evaluated on vertical or horizontal form-fill-seal equipment. Seal initiation is influenced by density, comonomer type, and surface additives. Because the resin has a lower density than a 0.930 g/cm³ medium-density grade, it can initiate seals at a lower jaw temperature, which may reduce energy consumption or allow higher line speeds. Seal strength is measured according to ASTM F88; hot-tack strength may be measured according to ASTM F2029. The operating window for seal temperature is not determined by density alone, because additive migration or surface roughness can shift the minimum seal temperature by several degrees. In coextruded films, the sealant layer often contains this resin because its octene comonomer contributes to seal strength and low-temperature durability, while an outer layer of higher-density polyethylene provides stiffness and temperature resistance.
Slip and antiblock additives migrate to the film surface over time. Erucamide-based slip agents reduce coefficient of friction but can alter seal contamination; the rate of migration is governed by diffusion through the amorphous phase. At typical warehouse temperatures, equilibrium surface concentration may require 24 to 72 h after extrusion. This ageing period should be included in packaging line trials. Coefficient of friction is measured according to ASTM D1894, and seal strength should be rechecked after ageing. For lamination or printing, corona treatment is commonly used to raise film surface energy to 38–42 dyn/cm; treatment decay occurs over time due to migration of low-molecular-weight species from the bulk, so surface energy should be measured at point of use according to ASTM D2578. Published data for this specific configuration is limited in open literature, so these ranges reflect typical converting practice rather than guaranteed values.
At equivalent density and melt index, ELITE™ 5110G differs from conventional Ziegler-Natta LLDPE primarily in comonomer placement and molecular weight distribution. Ziegler-Natta catalysts produce a heterogeneous distribution in which the low-molecular-weight fraction contains a higher concentration of comonomer. This creates a low-melting extractable fraction and reduces the effective crystallinity of the film. In ELITE™ 5110G, the single-site catalyst places 1-octene more evenly along the polymer chains. The result is fewer highly branched low-molecular-weight chains, a sharper melting endotherm, and lower extractable content as measured by regulatory extraction methods. The practical consequence is improved dart impact at equal film gauge and better organoleptics in food-contact applications.
Compared with a narrow molecular weight metallocene LLDPE, the difference is subtler. A very narrow molecular weight distribution can reduce melt strength and make the bubble more sensitive to air-ring turbulence. ELITE™ 5110G is designed with a controlled long-chain branching content that increases shear thinning and extensional hardening. This maintains bubble stability without recreating the high extractable fraction of Ziegler-Natta resins. On a production-scale line, the resin may exhibit a broader stable operating window than a narrow molecular weight metallocene grade at high blow-up ratios, but film clarity may be slightly lower than an optimized metallocene cast-film grade. Direct comparison requires the same die, tower, gauge, and cooling history.
| Attribute | Test basis | ELITE™ 5110G relative to Ziegler-Natta LLDPE of equal MI/density | ELITE™ 5110G relative to narrow-MWD metallocene LLDPE |
|---|---|---|---|
| Comonomer distribution | Thermal fractionation | narrower | comparable |
| Long-chain branching | Rheology | higher shear thinning | controlled population |
| Dart impact at equal gauge | ASTM D1709 | higher | film-dependent |
| Extractables | FDA 21 CFR 177.1520 extraction | lower | comparable |
The directional differences in the table are based on typical blown-film fabrication experience and standard characterization methods. They are not substitutes for line-specific comparative data. Any comparison must be made using the same die, tower, and gauge to avoid confounding geometry and cooling history.
For food-contact uses, the resin is typically manufactured to meet the compositional requirements of FDA 21 CFR 177.1520 for olefin polymers. Compliance under EU 10/2011 is evaluated on the final article, with migration testing conducted according to food type and contact conditions. Because migration kinetics in polymer matrices depend on film thickness, time, and temperature, density and melt index alone do not establish compliance for any specific food type. A food-contact statement from the manufacturer should be obtained for the specific additive package and intended use condition.
In non-food heavy-duty packaging, the main long-term limitation is oxidative stability under ultraviolet exposure. Polyethylene photo-oxidation reduces elongation at break and can cause film embrittlement. If outdoor storage is required, the converter must add a UV stabilizer masterbatch and validate weatherability according to ASTM D1435 or ISO 4892-2. The resin should not be stored in direct sunlight or high-temperature warehouses for prolonged periods because the antioxidant package may be consumed. It is also not recommended for hot-fill applications above 100 °C or for continuous contact with strong oxidizing agents.
The final application boundary occurs in industrial packaging lines running very thin films below 15 µm at high speed. In this regime, bubble cooling demand can exceed air-ring capacity, and the operator may observe gel streaks or gauge bands. The product can still be used if internal bubble cooling and automatic gauge control are available; otherwise, a higher melt index resin may be required to maintain bubble stability at extreme outputs.