| HS Code | 628174 |
| Chemical Family | Linear Low Density Polyethylene (LLDPE) |
| Density | 0.920 g/cm3 |
| Melt Index | 0.85 g/10 min (190 °C/2.16 kg) |
| Melt Flow Ratio | 8.0 (I10/I2) |
| Melting Point | 123 °C |
| Vicat Softening Point | 104 °C |
| Tensile Strength At Yield | 9.7 MPa |
| Tensile Strength At Break | 26 MPa |
| Elongation At Break | 700% |
| Dart Drop Impact | 250 g |
| Elmendorf Tear Md | 250 g |
| Elmendorf Tear Td | 350 g |
| Haze | 8% |
| Gloss 45 Degrees | 65 |
| Coefficient Of Friction | 0.2 |
| Low Temperature Brittleness | -70 °C |
As an accredited Dow ELITE™ 5100 Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Dow ELITE™ 5100 Linear Low Density Polyethylene is supplied in 25 kg polyethylene bags, typically stacked and shipped on pallets. |
| Container Loading (20′ FCL) | Dow ELITE™ 5100 Linear Low Density Polyethylene loaded in a 20′ FCL in palletized bags, securely stowed for ocean freight. |
| Shipping | Dow ELITE 5100 Linear Low Density Polyethylene ships as a non-hazardous polymer resin, typically in 25 kg bags on stretch-wrapped pallets or in bulk trucks/railcars. Keep dry, clean, cool, and away from direct sunlight and ignition sources. No UN hazard class or special transport labeling required. |
| Storage | Store Dow ELITE™ 5100 Linear Low Density Polyethylene in a cool, dry, well-ventilated area, away from direct sunlight, heat, sparks, flames, and strong oxidizers. Keep bags or containers closed, clean, dry, and palletized to prevent moisture, dust, and contamination. Avoid excessive stacking, high temperatures, and prolonged UV exposure. Follow the manufacturer’s SDS and local regulations; use first-in, first-out inventory. |
| Shelf Life | Recommended shelf life: 24 months when stored in original, unopened packaging in a cool, dry area away from direct sunlight. |
FFS sack converting for polymer pellets, fertilizer, and dry pet food subjects the film to sudden inflation at fill rates up to 1,800 sacks/h and to pinch-seal impulse cycles at the bottom fold. In this segment, ELITE 5100 is blended at 75–85 wt% with 15–25 wt% high-pressure LDPE having a melt index of 0.25–0.35 g/10 min; 2–3 wt% of a 20% silica antiblock masterbatch is added to hold the coefficient of friction between 0.25 and 0.35 per ASTM D1894. Erucamide slip is dosed at 500–1,000 ppm in the seal layer only to control blocking without reducing heat-seal strength below acceptance limits. The resin is processed on a three-layer blown film line with extruder diameters of 65 mm, 90 mm, and 55 mm, each with L/D 30:1; a 250 mm spiral mandrel die with a 2.0 mm die gap feeds a dual-lip air ring and internal bubble cooling. Melt temperature is held at 199–210 °C, and blow-up ratio is controlled at 2.0:1–2.5:1. The collapsed bubble with gusseted edges is produced at 150–200 µm thickness. Downstream conversion requires jaw temperature of 130–150 °C, seal dwell of 50–80 ms, and fill head pressure sufficient to densify 25 kg of product without rupturing the gusset fold. Thickness variation across the web is controlled by segmented die thermal expansion to ±5 µm because seal failure at thin points is the main documented field failure on FFS converting lines.
Finished sack compliance is verified against ASTM D5276-98(2018) drop testing for filled sacks, ASTM D1709-16a dart impact, and ASTM D1922 Elmendorf tear. For dry food packaging, resin compliance is governed by FDA 21 CFR 177.1520(c) 3.2 and EU Regulation 10/2011 with overall migration below 10 mg/dm² under dry contact conditions. Terminal products include 25 kg resin and fertilizer sacks, 10–20 kg pet food bags, and 50 kg industrial mineral bags.
At frozen filling temperatures below −25 °C, LLDPE film stiffness rises and the ductile-to-brittle transition moves closer to the operating window; ELITE 5100 is therefore placed in the sealant and core layers of three-layer coextruded frozen food film. The layer distribution is typically 30 wt% outer skin, 50 wt% core, and 20 wt% sealant. The outer skin is composed of 70 wt% ELITE 5100 and 30 wt% LDPE, the core of 90 wt% ELITE 5100 and 10 wt% LDPE, and the sealant of 98 wt% ELITE 5100 with 2 wt% antiblock masterbatch. This gives a total ELITE 5100 content of approximately 79 wt% in the film. Seal initiation is measured from 102 °C to 110 °C at 0.5 s dwell on a laboratory sealer.Extrusion uses a 250 mm three-layer blown film die with a 1.8 mm die gap and blow-up ratio of 2.5:1–3.0:1. Melt temperature is capped at 188–205 °C to limit gel formation from edge trim and to maintain the molecular weight distribution of the resin. The frost line is raised to 60–70 cm above the die to increase machine-direction tear strength; corona treatment is set to 38–42 mN/m per ASTM D2578 for water-based ink adhesion. Vertical form-fill-seal machines operate at 80–120 bags/min with seal jaw temperatures of 120–140 °C, dwell times of 30–50 ms, and pneumatic jaw pressure of 0.3–0.5 MPa. Low-temperature dart impact is the primary release criterion because the package is handled at freezer mezzanine temperatures below −18 °C.
Food contact compliance for the olefin layers is assigned to FDA 21 CFR 177.1520(c) 3.2, with EU Regulation 10/2011 requiring overall migration below 10 mg/dm² under frozen and chilled aqueous food simulants. If erucamide slip is used, its migration must be verified against the positive list and may not exceed the assigned SML in EU Regulation 10/2011. Terminal products include frozen vegetable pouches, par-fried potato bags, individually quick-frozen seafood bags, and frozen berry packs.
Laminated stand-up pouch converters specify ELITE 5100 in the cast sealant web because heat-seal strength must be retained after the laminate passes through solventless adhesive cure and pouch-making heat history. The sealant web is formulated at 85 wt% ELITE 5100, 10 wt% LDPE, and 5 wt% antiblock masterbatch. The layer thickness is 30–40 µm, and it is processed on a slot-die cast line with a die gap of 0.5–0.8 mm, chill-roll temperature of 22–26 °C, and line speed of 150–250 m/min. Corona treatment is applied immediately before lamination to reach a surface energy of 38–44 mN/m per ASTM D2578.
Heat-seal performance is quantified with ASTM F88/F88M at a jaw temperature of 130 °C, dwell of 0.2 s, and pressure of 0.3 MPa; typical seal strength exceeds 14 N/25 mm for a 40 µm sealant web. Hot tack measured per ASTM F1921/F1921M remains above 6 N/25 mm at 110 °C, which is the operating threshold for pouches filled through a bottom spout. The sealant web is adhesive-laminated to 12 µm PET or 18 µm BOPP and 7–9 µm aluminum foil using a solventless polyurethane adhesive at 1.5–2.0 g/m²; the laminate is cured at 45 °C for 48 h before slitting. Published data for seal initiation at high pouch-machine speeds is limited; each converter must verify the seal threshold on the actual machine because dwell time and jaw pressure vary by equipment supplier.
The sealant web meets FDA 21 CFR 177.1520(c) 3.2 for food contact under Conditions of Use A through G as appropriate for dry and aqueous acidic products. EU Regulation 10/2011 applies with overall migration below 10 mg/dm²; when the pouch contains rice, snack foods, or dry pet food, the converter verifies that the full laminate and adhesive system also comply with the relevant specific migration limits. Terminal products include stand-up pouches for snack foods, dry pet food, powdered beverage mixes, and detergent refill pouches.
Agricultural silage covers place severe puncture demands on the film because maize stalk ends and stem fragments propagate tears along the clamp edge during air evacuation and tyre weighting. ELITE 5100 is used at 82 wt% with 15 wt% LDPE and 3 wt% of a 20% carbon black/UV masterbatch, resulting in a carbon black concentration of 0.6 wt% in the finished film and reduced UV embrittlement over the 12–18 month storage period. Film thickness is maintained at 200–250 µm, and puncture resistance measured to ASTM D4833 is specified at not less than 400 N for a 200 µm film.
The film is produced on a monolayer or three-layer blown film line with a 350–500 mm die, die gap of 2.4–3.0 mm, and blow-up ratio of 1.8:1–2.2:1. The lower stalk height and melt temperature of 200–215 °C are maintained to reduce residual shrink that could pull the cover away from the clamp edge. The tube is edge-folded into lay-flat widths of 8–12 m and wound in 100–200 m rolls. Extruder output is limited to 350–450 kg/h because carbon black masterbatch increases melt viscosity and reduces bubble stability above this throughput. Published data for the exact combination of ELITE 5100 with HALS-stabilized carbon black masterbatch is limited, so converters run plant-scale weathering trials per ASTM G154 rather than extrapolating laboratory values.
In Europe, agricultural covering films are covered by EN 13206:2017 for dimensional and mechanical requirements; mechanical acceptance frequently references ASTM D4833 for puncture, ASTM D882 for tensile, and ISO 18553 for pigment dispersion. Terminal products include silage clamp covers, stack silage covers, and temporary pile covers for grain and chopped forage.
For liquid bag-in-box packaging, ELITE 5100 is placed in the polyethylene skins and heat-seal layer of five-layer EVOH barrier film used for 1–10 L liners. In a 65–90 µm structure, the sealant layer is formulated with 75 wt% ELITE 5100 and 25 wt% LDPE; the outer skin is formulated with 60 wt% ELITE 5100 and 40 wt% LDPE. The EVOH layer accounts for 4–6 µm of the total thickness, and maleic anhydride-grafted tie resin layers are 2–3 µm per side. Total ELITE 5100 content in the finished film is approximately 50–60 wt%, depending on tie layer and EVOH grade.The five-layer film is blown on a line with 45–65 mm extruders having L/D 30:1, a 200 mm spiral mandrel die, and die gap of 2.4 mm. Polyethylene melt temperatures are held at 200–210 °C; the EVOH melt stream is controlled at 215–230 °C to match the rheology of the adjacent tie layers. If ambient humidity in the converting hall exceeds 60% RH, the EVOH layer must be pre-dried or the oxygen transmission rate will exceed the target within 2 h of line start-up, a common barrier loss failure on five-layer blown film lines. Oxygen transmission rate after lamination and spout insertion is targeted below 1 cm³/(m²·day·atm) at 23 °C and 0% RH per ASTM D3985. The film is converted on bag-in-box fillers operating at 40–60 bags/min, with spout sealing performed by ultrasonic welding at 20 kHz and 0.5–1.5 s weld time.
The polyethylene layers comply with FDA 21 CFR 177.1520(c) 3.2; EVOH compliance is assigned to FDA 21 CFR 177.1360. EU Regulation 10/2011 applies with overall migration below 10 mg/dm² in aqueous and fatty food simulants appropriate to the packed liquid. Terminal products include bag-in-box liners for post-mix syrup, condiment sauces, edible oil, and wine; for wine, the converter verifies specific migration limits for the adhesive and tie layer system because the alcohol simulant is 10–20% ethanol.
Competitive Dow ELITE™ 5100 Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Dow ELITE™ 5100 Linear Low Density Polyethylene is an ethylene-octene copolymer produced on a solution polymerisation platform using constrained geometry catalyst technology. The resin is supplied in pellet form and is classified as a linear low density polyethylene because the short-chain branching arises from octene incorporation rather than from high-pressure radical polymerisation. Nominal density is 0.920 g/cm³ when tested in accordance with ASTM D1505-18, and nominal melt index is 0.85 g/10 min at 190°C/2.16 kg according to ASTM D1238-20. The same melt flow condition is reported under ISO 1133-1:2022 as a melt flow rate of 0.85 g/10 min. These values place the resin in the medium-density region for blown film LLDPE and at a melt index normally selected for medium-to-thick gauge film extrusion.
| Property | Test method | Representative value |
|---|---|---|
| Density | ASTM D1505-18 | 0.920 g/cm³ |
| Melt index | ASTM D1238-20 | 0.85 g/10 min |
| Melt flow rate | ISO 1133-1:2022 | 0.85 g/10 min |
The values in Table 1 are representative, not specification limits. The sales specification is agreed with the manufacturer and may include lot-to-lot control limits for melt index and density. Users should request the current product data sheet and certificate of analysis before making material substitutions. Molecular weight and comonomer distribution are not shown in the standard datasheet, but the manufacturer’s technical literature describes the resin as having a narrower short-chain branching distribution than conventional Ziegler-Natta butene-copolymer LLDPE. High-temperature gel permeation chromatography with differential refractive index detection, conducted under ISO 16014-4:2019, is used to verify lot-to-lot consistency of the molecular weight distribution. Differential scanning calorimetry according to ASTM D3418-21 is used to characterise the melting endotherm and crystallisation exotherm. The crystallisation temperature and heat of fusion are lot-dependent but are bounded by the nominal density specification. The practical consequence of the molecular architecture is a higher tie-chain population in the amorphous phase than is typical for butene-copolymer LLDPE at equivalent density, which influences solid-state tensile energy absorption and dart impact response.
The resin is not interchangeable with high-pressure low density polyethylene in rheological terms. Melt tension and extensional viscosity requirements in large-bubble film are different from those of high-pressure LDPE, and the shear-thinning index is moderate rather than strong. Converters evaluating the resin for replacement of a conventional butene-copolymer LLDPE should retain the same melt index comparison only when the same die gap, blow-up ratio, and frostline height are used; otherwise the comparison is confounded by orientation and cooling history.
Start-up conditions reported for similar 0.920 g/cm³, 0.85 g/10 min ethylene-octene copolymers on single-screw extruders begin with feed throat temperature of 40°C to 50°C and barrel setpoints from 180°C to 215°C. Adapter and die setpoints are commonly 215°C to 230°C. These settings are not universal; screw diameter, barrier flight depth, compression ratio, and die gap change the shear heating contribution. The melt index of 0.85 g/10 min indicates a larger molecular weight than general-purpose LLDPE with melt indices above 1.0 g/10 min, so melt pressure at the breaker plate increases more rapidly with screw speed. On a 65 mm, 30:1 L/D grooved-feed extruder, typical melt pressure may rise from 180 bar at 60 min⁻¹ to 300 bar at 110 min⁻¹; published data for this specific configuration is limited, and the extruder manufacturer’s maximum pressure rating takes precedence. Melt temperature at the die should be kept below 245°C to limit oxidative chain scission and gel formation. Resin lot-to-lot variation in melt index can shift pressure by several bar, so incoming lot data should be compared against the supplier’s certificate of analysis before setting alarm limits.
Pressure stability is also affected by pellet conveying. Condensation on cold pellets introduced into a warm feed throat can produce pressure fluctuations and output surging. In high-humidity production halls, the pellet hopper should be purged with dry air and the feed throat temperature maintained at the low end of the stated range to avoid bridging. The screw should be run at a low speed during the first 15 min after start-up to establish a stable melt pool before increasing output. Film producers that operate at very high screw speeds should monitor specific energy consumption because shear heating in ELITE™ 5100 increases melt temperature faster than in a lower-viscosity butene-copolymer LLDPE with equivalent melt index.
The flow curve of ELITE™ 5100 is not described by melt index alone. Capillary rheometry at 190°C and 210°C over shear rates from 100 s⁻¹ to 1000 s⁻¹ is required to estimate die pressure drop and melt fracture onset. The resin’s narrow comonomer distribution and linear backbone produce a weaker shear-thinning response than high-pressure LDPE, but the melt retains enough viscosity at die entry to create vortices if the die gap is too wide or the land length is too short. Sharkskin and gross melt fracture are not resin properties alone; they depend on die entry angle, die land length, die surface roughness, and melt temperature. Die gaps below 1.0 mm and die land ratios greater than 10:1 are commonly used for LLDPE blown film to minimise melt fracture. The onset of sharkskin is typically shifted to higher shear rates when the die temperature is raised from 210°C to 230°C, but this also increases risk of thermal degradation. Validation of the operating boundary should be conducted on the specific die because laboratory capillary data do not capture the effect of temperature non-uniformity in the die body.
Film performance for Dow ELITE™ 5100 is evaluated after conditioning for 40 h at 23°C ± 2°C and 50% ± 5% RH according to ASTM D618-21. Dart impact is measured under ASTM D1709-16a Method A on films blown at a 2.5:1 blow-up ratio. Elmendorf tear is determined by ASTM D1922-15, and tensile properties by ASTM D882-18 at a jaw separation speed of 500 mm/min. Haze is measured by ASTM D1003-13, and 45° gloss by ASTM D2457-13. The product is used in heavy-duty shipping sacks, agricultural silage film, industrial liners, bag-in-box structures, and puncture-resistant overwrap. Typical finished film thickness is between 50 μm and 200 μm, depending on filled weight, puncture exposure, and sealing requirements. In these applications, the resin is selected because the octene-based short-chain branching increases transverse-direction tear and dart impact relative to butene-copolymer LLDPE at equivalent density. The film gauge can often be reduced while maintaining a specified dart impact limit; however, the reduction must be confirmed by ASTM D1709-16a on the production line, not inferred from laboratory data alone.
Machine-direction tear in blown film is predominantly orientation-controlled. The same resin may show a lower machine-direction tear after high stalk height or high drawdown. Converters should not expect equal machine-direction and transverse-direction tear values; anisotropy is governed by blow-up ratio, frostline height, and drawdown. At a blow-up ratio of 2.0:1, transverse-direction orientation is lower than at 3.0:1, shifting the tear balance. The resin’s practical property balance in heavy-duty sacks is commonly obtained at a blow-up ratio between 2.2:1 and 2.8:1, but this range must be validated on the production die and air ring.
Seal initiation temperature for ELITE™ 5100 is a function of density and comonomer type. Octene copolymers generally exhibit lower seal initiation than butene copolymers of equal density because the branches disrupt crystallite formation more effectively at the sealing surface. Hot tack is measured according to ASTM F1921-20 and heat seal strength according to ASTM F88/F88M-21. The resin is used in bag-in-box and heavy-duty sack sealing operations where seal integrity must be maintained after creasing or product loading. Converters should report seal bar temperature, sealing pressure, and dwell time when comparing lots; a change of 5°C in seal bar temperature can shift seal strength across the acceptance threshold in high-speed vertical form-fill-seal equipment. Published data for this specific configuration is limited.
Comparisons between ELITE™ 5100 and butene-copolymer LLDPE should be made at equal density and equal melt index. In conventional Ziegler-Natta butene LLDPE, the low-molecular-weight fraction is comonomer-rich, while the high-molecular-weight fraction is relatively linear. This broad intermolecular composition distribution produces a wide range of lamellar thicknesses and leaves fewer stress-transmitting tie molecules in the amorphous phase. ELITE™ 5100 is designed to narrow the composition distribution and place more comonomer on the high-molecular-weight fraction. The effect is measurable as higher dart impact in ASTM D1709-16a and higher transverse-direction Elmendorf tear in ASTM D1922-15 at equivalent film thickness and density. The difference is smaller in machine-direction tear, where melt orientation dominates, and in low-speed tensile yield, where crystallinity and lamellar continuity dominate. The resin also differs from high-pressure LDPE in melt tension and strain-hardening behaviour; it is less extensional-thinned and should not be assumed to provide the same bubble stability in high-stalk film. Blends of ELITE™ 5100 with LDPE should be evaluated on the production line for melt curtain stability and transverse-direction tear attenuation.
Compared with some metallocene hexene or octene LLDPE grades, ELITE™ 5100 may exhibit a broader molecular weight distribution that improves bubble stability and reduces melt fracture but may sacrifice ultimate optical clarity. Published data for this specific comparison is limited and is dependent on the selected metallocene reference grade.
Manufacturer documentation refers to the food-contact status of ELITE™ 5100 under a range of regulatory frameworks. The designations in Table 2 are those commonly cited for olefin polymers and are not a substitute for finished-package migration testing. For multi-layer films, the converter must establish whether the food-contact layer is separated by a functional barrier and select worst-case food simulants. In dangerous-goods packaging, drop and stack performance is governed by UN 6.1.5 and national transport regulations; the resin must be accompanied by a certificate of analysis for melt index and density to support traceability. No medical implant or pharmaceutical packaging claims are made in the manufacturer’s unpublished technical literature.
| Regulatory framework | Designation | Applicability |
|---|---|---|
| U.S. Food and Drug Administration | 21 CFR 177.1520 | Olefin polymers in contact with food, subject to migration limits |
| European Union food contact | Regulation (EU) No 10/2011 | Plastic materials and articles intended to come into contact with food |
| Hazard communication | GHS classification | Not classified as hazardous according to supplier safety data sheet |
| REACH polymer registration | Regulation (EC) No 1907/2006 | Polymers are exempt from registration; monomers and additives remain subject to registration |
No pre-drying is normally required for ELITE™ 5100 pellets stored in sealed containers at ambient temperatures below 30°C and relative humidity below 60%. If pellets are transferred from an unheated warehouse into a warm production hall, sealed packaging should be allowed to reach room temperature before opening to prevent condensation. Surface moisture above 0.02% by mass can generate steam splay in film above 100 μm and destabilise the melt pressure reading. Regrind addition up to 20% by mass is common in non-critical heavy-duty sacks, but the proportion must be validated against dart impact and transverse-direction tear because thermal history shifts the molecular weight distribution and lowers fractional crystallinity. Ultraviolet stabilisation is required for long-term agricultural exposure; the resin as supplied is not formulated for outdoor weathering beyond typical warehouse storage. Accelerated weathering in ASTM G155-21 xenon-arc testing is used for formulation screening but does not replace outdoor exposure in the target climate. Additive packages containing high levels of low-molecular-weight amines should be evaluated for organoleptic interaction in sensitive food-contact film. The product is not recommended for use in medical implants, and no statement of fitness for such use is provided by the manufacturer.