| HS Code | 479988 |
| Density | 0.921 g/cm3 |
| Melt Index 190 C 2 16 Kg | 0.90 g/10 min |
| Melt Flow Ratio I21 I2 | 27 |
| Melting Point | 122 °C |
| Vicat Softening Temperature | 98 °C |
| Tensile Strength At Yield | 10 MPa |
| Tensile Strength At Break | 30 MPa |
| Elongation At Break | 800% |
| Flexural Modulus | 240 MPa |
| Dart Impact Strength | 200 g |
| Elmendorf Tear Strength Md | 300 g |
| Elmendorf Tear Strength Td | 500 g |
| Haze | 12% |
| Gloss 45 | 55 |
| Coefficient Of Friction | 0.20 |
As an accredited Dow DOWLEX™ 3010 Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | DOWLEX™ 3010 is supplied in 25 kg polyethylene-lined bags, palletized at 1,000 kg net weight per pallet. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): about 18–20 MT of Dow DOWLEX™ 3010 LLDPE in 25 kg bags, palletized or floor-loaded. |
| Shipping | DOWLEX™ 3010 LLDPE is shipped as non-hazardous solid resin pellets in sealed moisture-barrier bags, octabins, or bulk trucks/railcars. Store cool and dry, away from direct sunlight, heat, moisture, and contaminants. Not classified as dangerous goods for transport; avoid prolonged UV exposure. |
| Storage | Store DOWLEX™ 3010 LLDPE in original, sealed packaging in a clean, dry, well-ventilated area. Protect from direct sunlight, moisture, heat, dust, and contamination. Keep away from ignition sources and strong oxidizers. Maintain moderate temperatures, avoid excessive stacking, and use stock rotation. Do not store outdoors or near incompatible materials. Ensure containers remain closed and labeled. Follow SDS and local regulations. |
| Shelf Life | DOWLEX™ 3010 LLDPE has no fixed shelf life; store cool, dry, away from sunlight and heat for long-term stability. |
Heavy-duty industrial liners and shipping sacks converted from DOWLEX™ 3010 are typically extruded on monolayer or three-layer blown-film lines. The resin is characterized by a nominal density of 0.921 g/cm³ under ISO 1183-1:2019 and a melt mass-flow rate of 1.0 g/10 min at 190 °C with 2.16 kg load under ISO 1133-1:2022. Single-screw extruders with barrier screws and Maddock mixing sections are used at L/D 24:1 to 30:1; barrel zones are profiled from 160 °C at the feed throat to 215 °C at the adapter, while die melt temperature is held between 199 °C and 227 °C. The annular die gap is maintained at 1.5 mm to 2.5 mm, with blow-up ratios from 2.0:1 to 3.0:1 on high-stalk bubble configurations. This combination is required because the narrow molecular-weight distribution of LLDPE produces lower melt strength than autoclave LDPE and cannot sustain extreme bubble geometry without flutter, particularly at film thickness below 50 µm.
The bubble stability threshold is governed by both frost line height and die output rate. At die lip exit velocities above approximately 1.2 kg/h per mm of die circumference, sharkskin or surface melt fracture appears unless a fluoropolymer processing aid is compounded at 200 ppm to 500 ppm by weight. As an alternative or in addition, LDPE is blended at 10 wt% to 20 wt% to introduce long-chain branching and stiffen the melt; above 30 wt% LDPE, machine-direction Elmendorf tear measured under ASTM D1922-15 usually falls because the oriented LLDPE crystal network is diluted. The collapsing frame, nip roll, and winding tension are set so that film thickness variation remains within ±5% of target; on high-speed form-fill-seal lines, variation exceeding ±8% correlates with bag side-seal failures. Surface condensation during cold-warehouse-to-plant transfer at relative humidity above 60% requires a hopper dryer at 70 °C for 2 h; polyethylene is not hygroscopic, but water films on pellets cause screw slip and pressure fluctuation.
Mechanical acceptance for industrial liners typically uses ASTM D882-18 for tensile and elongation, ASTM D1709-15a for dart impact, ASTM D1922-15 for Elmendorf tear, ASTM D1003-13 for haze, and ASTM D1894-14 for coefficient of friction. Because product specifications vary by fill weight and automatic sack-opening equipment, a single universal dart-impact limit is not available; converters monitor a minimum Cpk of 1.33 against internal specification limits derived from end-user line trials. Film blocking is addressed with synthetic silica anti-block at 2,000 ppm to 5,000 ppm, and coefficient of friction is modified with erucamide slip additive at 500 ppm to 1,000 ppm; these additive ranges must be reviewed against food-contact status under FDA 21 CFR § 177.1520 and EU 10/2011 when the sack is used for indirect food contact.
| Converting operation | Primary normative reference | Critical test method | Acceptance basis |
|---|---|---|---|
| Heavy-duty industrial liners | FDA 21 CFR § 177.1520, EU 10/2011 | ASTM D882-18, ASTM D1709-15a, ASTM D1922-15 | Cpk ≥ 1.33 against converter internal limits |
| Silage wrap | EN 13206 | ISO 527-3, ISO 6383-2, ISO 7765-1 | 12-month to 18-month UV weathering |
| Cast stretch film | ASTM D5458 | ASTM D1894-14, ASTM D882-18 | Cling force and stretch retention at 200% to 300% |
| Geomembrane | GRI-GM13 | ASTM D6693, ASTM D4833, ASTM D5397 | Project-specific puncture and SP-NCTL |
| Injection molded closures | ISO 294-1 | ISO 180, ISO 527-2, ASTM D1693 | Dimensional stability and ESCR |
| Extrusion coating | FDA 21 CFR § 177.1520, EU 10/2011 | ASTM F88/F88M-15, ASTM D1894-14, TAPPI T 540 | Seal strength and adhesion |
Silage wrap made from DOWLEX™ 3010 is typically produced as a 25 µm monolayer or coextruded blown film in widths between 500 mm and 750 mm. The operational conflict involves frost line height: a frost line raised to 4 to 8 times the die diameter raises machine-direction orientation and therefore increases machine-direction tensile modulus under ISO 527-3, but simultaneously reduces transverse-direction Elmendorf tear under ISO 6383-2. In silage baling, transverse-direction tear is not a secondary property; it is the primary buffer against stalk puncture when bales are wrapped under tension. The processing window is therefore narrow, with frost line adjustment often limited to ±5% of the nominal height before tear balance moves outside the specification band.
UV stabilization is incorporated at 0.25 wt% to 0.60 wt% of a high-molecular-weight hindered amine light stabilizer package, frequently combined with 0.10 wt% to 0.20 wt% of a benzotriazole UV absorber for a service life of 12 to 18 months outdoor exposure. Titanium dioxide is used at 2 wt% to 4 wt% for opacity and UV screening, but loadings above 5 wt% increase melt viscosity and may initiate surface melt fracture at the die exit. The film is produced on high-stalk bubble lines with internal bubble cooling and a sizing cage; the air flow to the internal bubble cooling system is adjusted before die throughput is increased, because LLDPE cannot tolerate simultaneous step changes in melt temperature and frost line height without bubble instability.
Testing under EN 13206 covers tensile properties, tear resistance, dart impact, and UV aging. For converter release, film is also tested under ISO 527-3 for tensile stress at break in both directions, ISO 6383-2 for trouser tear, ISO 7765-1 for dart impact, and ISO 4892-2 for accelerated weathering. Field failures in silage film are commonly traced to gel streaks formed during long runs at high output; a screen pack of 60/100/60 mesh is therefore installed before the die, with back pressure monitored against a baseline value at constant screw speed. A pressure rise above 15% during a 24 h run indicates gel accumulation and requires a screen change before film enters the baling market.
Cast pallet wrap using DOWLEX™ 3010 as a core layer is processed through a slot die with automated die-lip heaters, an air knife, and a polished chill roll. The melt temperature at the die is held between 249 °C and 282 °C; die gap is typically 0.38 mm to 0.76 mm; and the air gap between die lip and chill roll is maintained under 100 mm to limit neck-in before the sheet touches the chill roll. The chill roll temperature is controlled at 18 °C to 30 °C. Draw ratios of 20:1 to 30:1 between die gap and final film thickness are normal, but draw resonance appears as transverse thickness bands when the draw ratio exceeds the melt strength boundary for a given line speed; the condition usually begins at film thickness below 10 µm and is suppressed by adding 10 wt% to 20 wt% LDPE or by increasing the air-gap cooling. For a 20 µm core layer, line speed is typically limited by edge trim handling and winder tension rather than by the extruder output.
Cling performance is not built into the core layer; it is supplied by metallocene-catalyzed ULDPE or polyisobutylene-based cling layers in a three-layer coextrusion. DOWLEX™ 3010 contributes the puncture resistance and load retention in the core. Stretch force and stretch retention are measured under ASTM D5458, coefficient of friction under ASTM D1894-14, and tensile elongation under ASTM D882-18. Roll conformity risk arises from built-in stress across the web; if chill roll temperature varies by more than ±3 °C across the width, the resulting differential crystallization creates telescoping on the finished roll during pre-stretch at 200% to 300% elongation. Batch-to-batch variation in melt mass-flow rate should be maintained within ±0.1 g/10 min to avoid visible die-line changes on the primary slitting lanes.
| Processing or formulation adjustment | Typical loading / setting | Observed effect | Boundary condition |
|---|---|---|---|
| LDPE blend in blown and cast film | 10 wt% to 20 wt% | Bubble stabilization, draw resonance suppression | Above 30 wt% may reduce dart impact |
| Fluoropolymer processing aid | 200 ppm to 500 ppm | Suppression of sharkskin at high output | Above 800 ppm can produce die drool |
| Erucamide slip additive | 500 ppm to 1,000 ppm | Reduction in coefficient of friction | Above 1,000 ppm plate-out on rolls |
| Synthetic silica anti-block | 2,000 ppm to 5,000 ppm | Blocking resistance in film rolls | Above 5,000 ppm raises haze |
| Hindered amine light stabilizer package | 0.25 wt% to 0.60 wt% | Silage wrap weathering resistance | Below 0.20 wt% can lead to premature cracking |
| Titanium dioxide | 2 wt% to 4 wt% | Opacity and UV screening | Above 5 wt% increases melt fracture risk |
DOWLEX™ 3010 can be specified in geomembrane sheet extrusion where a flexible LLDPE liner is required for secondary containment, canal lining, or landfill caps. The main process conflict is the low-shear melt fracture boundary at the sheet die. Extruders are typically single-screw machines with L/D 30:1 or twin-screw compounding lines feeding a coat-hanger sheet die, but the die gap must be kept above 2.0 mm. If the die gap is reduced below 1.8 mm to achieve faster gauge changeover, the linear polymer exhibits sharkskin at the die lip even at moderate throughput because wall shear stress in the die lip exceeds the critical value for spurt flow. The melt temperature is held between 218 °C and 249 °C; lower temperatures raise melt viscosity and shift the fracture threshold to even lower line speeds.
Sheet thickness for LLDPE geomembranes normally ranges from 0.75 mm to 2.0 mm, produced through a three-roll stack with roll temperatures between 60 °C and 90 °C. The roll gap is set to maintain embossing depth without creating gauge variation. The draw ratio between die gap and finished sheet is kept low, 1.5:1 to 2.5:1, because LLDPE has limited melt strength for free-web stretching; excessive draw creates transverse caliper variation and edge bead thickness. Published data for this specific grade in textured geomembrane configuration is limited; converter validation therefore includes a short-run capability study using ASTM D4439 material classification, ASTM D6693 tensile stress at yield and break, ASTM D4833 puncture resistance, ASTM D5397 notched constant tensile load, and GRI-GM13 project specifications.
Seaming compatibility is a practical limitation: LLDPE geomembrane panels are hot-wedge welded or fusion welded at temperatures lower than HDPE. If the welding wedge temperature is set using an HDPE profile, the LLDPE sheet can exhibit localized thinning at the seam edge; the correct wedge temperature is usually 10 °C to 20 °C lower than that used for HDPE. Weld peel and shear tests are conducted in accordance with GRI-GM19. The low density of DOWLEX™ 3010 leads to higher flexibility and lower stiffness than HDPE, but it also reduces resistance to sustained tensile load under ASTM D5397; project specifications for landfill caps may require a higher-density LLDPE or HDPE if long-term stress cracking is the controlling failure mode. For this reason, DOWLEX™ 3010 is not a general substitute for all geomembrane resins and is selected only after site-specific chemical compatibility and stress-cracking review.
In flexible overcaps and living hinges, DOWLEX™ 3010 is injection molded only where the end user has validated the grade for thin-wall applications, because the resin is not a dedicated injection-molding grade. Melt temperature is profiled from 190 °C at the feed to 232 °C at the nozzle, and mold temperature is maintained between 15 °C and 40 °C. For caps with wall sections of 1.0 mm to 2.0 mm, injection velocity is set high enough to prevent freeze-off before the flow front reaches the hinge, but excessive velocity causes jetting in the hinge area. A gate diameter of 0.8 mm to 1.5 mm is used for thin-wall overcaps, and because LLDPE has a relatively slow crystallization rate compared with HDPE, the cooling time is longer; cycle-to-cycle variation in cooling-water temperature above ±2 °C creates hinge stress that may crack after repeated flexing under ISO 178 or ASTM D790.
The low density of 0.921 g/cm³ gives lower flexural modulus and softer snap-fit insertion than polypropylene or HDPE; this can be advantageous for tamper-evident overcaps and child-resistant closures. However, low modulus also means that continuous load-bearing threads may deform if the closure is torqued beyond the design limit. The material is tested for environmental stress cracking resistance under ASTM D1693 or ISO 22088-3 when closures are used with aggressive liquid packaging. Dimensional stability is verified by molding specimens under ISO 294-1 and measuring shrinkage after 24 h at 23 °C ± 2 °C and 50% ± 5% relative humidity. Molded part shrinkage for this grade is generally higher than that of a propylene impact copolymer, so the tool is cut to a larger initial cavity dimension and adjusted after first-article dimensional inspection. Published rheological data for DOWLEX™ 3010 in injection molding is limited; mold fill simulation should use capillary rheometry data measured on the actual lot rather than software default databases.
Extrusion coating with DOWLEX™ 3010 requires a higher melt temperature than blown film to promote wetting and adhesion to paperboard, aluminum foil, or oriented polyester film. Melt temperature at the die is held between 288 °C and 316 °C, and the die gap is set to 0.5 mm to 0.8 mm. The air gap between flat die and nip into the chill roll is controlled between 150 mm and 250 mm; longer air gaps increase neck-in and reduce effective coating width, while shorter air gaps reduce time available for surface oxidation and cut adhesion strength. The chill roll is polished and maintained at 10 °C to 20 °C to quench the coating and control crystallinity. Coating weights for liquid packaging structures typically range from 15 g/m² to 40 g/m². At these coating weights, the primary film defect is draw resonance only when line speed exceeds the melt strength boundary; adding 10 wt% to 20 wt% LDPE is the standard correction.
The adhesion mechanism in extrusion coating is not a solvent or primer bond; it relies on oxygen-containing polar species formed at the melt surface during the air gap. Ozone treatment of the molten web at 2 g/h to 4 g/h per meter of width can be used when lower melt temperatures are required or when adhesion to foil must be raised. However, excessive ozone or melt temperature above 320 °C produces oxidative degradation by-products that carry into packaged liquids as off-taste. Heat seal strength is measured under ASTM F88/F88M-15, and the heat seal initiation temperature is typically recorded during a pressure-impulse heat sealer calibration. For food-contact use, the coated structure is evaluated under FDA 21 CFR § 177.1520 for the olefin polymer component and under EU 10/2011 for overall migration; the additive package used in extrusion coating must not include slip or anti-block concentrates that exceed the migration limits for the intended food simulant.
When DOWLEX™ 3010 is substituted for LDPE in a liquid packaging coating layer, the converter should expect lower melt strength and greater neck-in under the same die gap and air gap, which reduces usable coating width. The die edge bead is heavier and must be trimmed. The lower density also reduces stiffness of the coating, which can alter finished cup rim stiffness and sealing bar release; barrier properties remain governed by the foil or metallized substrate, not by the polyethylene layer. Therefore, outlet test methods include ASTM D1894-14 for coefficient of friction, ASTM D1922-15 for tear resistance of the laminated structure, and TAPPI T 540 for simulated peel testing in production. Because the resin grade is not specifically marketed for every coating line, converter-run capability data is required before changing from a conventional autoclave LDPE.
Competitive Dow DOWLEX™ 3010 Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
DOWLEX™ 3010 Linear Low Density Polyethylene is a solution-polymerized ethylene-octene copolymer supplied as pelletized resin. Manufacturer data list a density of 0.918 g/cm³ under ASTM D792 and a melt index of 1.0 g/10 min under ASTM D1238 at 190 °C/2.16 kg. A corresponding melt mass-flow rate may be reported under ISO 1133-1:2022. The resin is positioned in the DOWLEX family for cast film extrusion because its linear backbone and hexyl short-chain branches give a balance of drawdown, tear resistance, and heat-seal response that differs from conventional butene-based linear low density polyethylene and autoclave low density polyethylene. The grade is a base polymer rather than a ready-to-use compound; it contains processing stabilizers but no slip, antiblock, or polymer processing aid. Additive loading for film-surface performance is introduced by converter masterbatch dilution. The material is not predried under normal storage conditions, although condensation on cold pellets moved into a warm processing hall can produce surface defects. Melt index and density are the two lot-level parameters typically controlled on certificates of analysis; variation in these bulk values is narrow but does not capture the branch-length distribution that defines the product.
In thicknesses from 12 µm to 50 µm, DOWLEX 3010 is used in industrial stretch wrap, food packaging overwrap, and lamination sealant webs where room-temperature stretch retention and tear propagation resistance are specified. The primary conversion route is cast film extrusion. Blown film use is possible, but the quench-dominated cast morphology is the customary route to low haze and balanced machine-direction/transverse-direction shrinkage. On high-speed stretch-wrap lines, the film is pre-stretched through motorized rollers to elongation ratios that often exceed 200%; the resulting tensile energy absorption is therefore more relevant than the low-strain modulus alone. Standard tensile testing under ASTM D882 and puncture testing under ASTM D5748 are used to compare lots, but the converter often measures film performance on the actual pre-stretch unit because laboratory elongation at break does not directly predict field failure at high elongation rates. Published data for DOWLEX 3010 at commercial pre-stretch speeds above 400 m/min are limited; trials on the target line are required.
In linear low density polyethylene, the comonomer branch length controls the relationship between crystallinity and tie-chain formation. Butene comonomer inserts ethyl branches of two carbon atoms; octene inserts hexyl branches of six carbon atoms. Because the hexyl branch more effectively disturbs crystal lamellae per branch point, an octene-based LLDPE can reach a given density with a higher level of mechanical connectivity in the amorphous regions. This is one reason why the Elmendorf tear strength measured under ASTM D1922 and the dart drop impact measured under ASTM D1709A are typically higher for DOWLEX 3010 than for a butene-based LLDPE of identical density and melt index. The effect is directional: on cast film, the tear test reports separate machine-direction and transverse-direction values, and the balance changes with draw ratio. An increase in machine-direction orientation generally lowers machine-direction Elmendorf tear while increasing transverse-direction tensile strength. The converter therefore controls the quench and take-off speed to keep the film isotropic enough for the application. Gel permeation chromatography with infrared detection confirms that the comonomer in DOWLEX 3010 is concentrated in the high-molar-mass fraction; this population is responsible for load transfer across amorphous boundaries. Bulk density and melt index do not reveal this distribution, which is why two resins with identical 0.918 g/cm³ density and 1.0 g/10 min melt index can show different film toughness.
Cast film extrusion of DOWLEX 3010 on single-screw extruders is conventionally run with barrel temperatures from 190 °C in the feed zone to 265 °C in the metering zone, with the die and adaptor maintained at 260 °C to 290 °C. Processors using 75 mm to 120 mm extruders with 30:1 L/D and barrier screws report stable plastication when the feed throat is kept below 50 °C. A flat die with a nominal gap of 0.8 mm to 1.2 mm is used; final gauge is then set by the primary chill-roll haul-off speed. The primary roll is held at 15 °C to 25 °C, and secondary rolls remove residual heat. Weak air-knife pinning or a worn die lip can produce transverse-thickness oscillation and optical defects. Above approximately 250 m/min, the melt curtain may enter draw resonance if the die gap is too small or the melt temperature is too low; increased melt temperature reduces viscosity but also lowers melt strength, so line-speed optimization is not monotonic. Die lip fouling and internal gel formation are monitored by pressure rise across the screen pack; a rise of more than 10% from the stable start-up value is a common trigger for screen replacement. Fluoroelastomer polymer processing aid at 0.02% to 0.06% by weight may be added if sharkskin surface melt fracture persists at production output. This film roughness is a die-lip stress phenomenon, distinct from particulate gel contamination, and requires a different remedy.
Chill-roll temperature is a primary determinant of quench rate and therefore of crystalline morphology in cast film. A rise of more than 3 °C in the primary roll during a production run changes the lamellar thickness distribution and can reduce the room-temperature extensibility of thin-gauge DOWLEX 3010 film even when the melt temperature and line speed are unchanged. The effect is most evident in films thicker than 40 µm, where the core cools more slowly and the morphology becomes less uniform through the film thickness. Under these conditions, dart impact measured under ASTM D1709A and puncture resistance measured under ASTM D5748 may shift by a detectable but lot-dependent amount, while haze and gloss remain within specification. The operator should log coolant inlet temperature, primary roll inlet and outlet temperatures, and line speed for every lot. Batch-to-batch differences in crystallization kinetics are generally smaller than the effect of roll-temperature drift exceeding this threshold. Because the product is intended for high pre-stretch stretch wrap, a loss of extensibility caused by slow quench is not recoverable by adjusting melt temperature alone; the roll temperature must be corrected and the affected film segregated for lower-stretch applications.
In flexible packaging sealant webs, the choice among autoclave low density polyethylene, butene-based linear low density polyethylene, and DOWLEX 3010 is driven by seal initiation temperature, hot-tack plateau, and tear performance. Autoclave LDPE has long-chain branching and broad molecular weight distribution, which provide high melt strength and neck-in resistance but produce a lower plateau modulus and lower tear resistance in oriented films than an octene-based LLDPE of similar density. Butene-based LLDPE of identical density and melt index has a higher branch frequency over the entire composition range but shorter branch length; this reduces its ability to resist crack growth in oriented films. DOWLEX 3010 differs by combining a linear backbone with longer hexyl branches. This combination lowers the melting peak below that of a high-density polyethylene but retains a narrower melting endotherm than an autoclave LDPE. In a sealant web, the practical result is that DOWLEX 3010 can produce a seal that develops strength within a narrower temperature window and withstands higher post-filling stress than a butene grade of similar sealing viscosity. The substitution of DOWLEX 3010 for a butene LLDPE on an existing cast line should not be made without checking the die-lip shear stress; the octene copolymer has a different shear viscosity at typical die shear rates, and the melt temperature or die gap may require adjustment to avoid an increase in gel-like surface defects. Converters also compare the extractables profile of the base resin and the formulated film, because the comonomer type and the stabilizer package influence the amount of low-molar-mass material that can migrate into fatty food simulants.
Food-contact suitability of articles made from DOWLEX 3010 is determined by the fabricated article, not by pellet-level data alone. The base resin may be used in single-layer and multilayer structures intended for food contact provided the converter verifies end-use conditions under the relevant regulatory frameworks. The following matrix lists the core citations commonly reviewed for this grade.
| Regulation or Standard | Citation | Assessment Focus |
|---|---|---|
| U.S. FDA food contact | 21 CFR 177.1520(c) 3.1a / 3.2a | Olefin polymers for contact with aqueous, acidic, and fatty foods |
| EU plastics regulation | EU Regulation (EU) No 10/2011, Annex I and II | Authorized monomers/additives and overall migration limit 10 mg/dm² |
| REACH | EC No 1907/2006, Annex XVII | Monomer and additive restrictions; no SVHC above 0.1% w/w |
| RoHS II | Directive 2011/65/EU Annex II | Lead 0.1%, cadmium 0.01%, mercury 0.1%, chromium VI 0.1%, PBB 0.1%, PBDE 0.1% by weight in homogeneous material |
The table does not replace migration testing. For fatty-food contact above 60 °C, published data for this specific configuration are limited; conversion should proceed only after extractables and overall migration testing under EU Regulation (EU) No 10/2011, Annex III and V, or under 21 CFR 177.1520(c) end-use conditions. The final article may also require national pesticide or pharmaceutical ordinances if used in medical packaging; those are outside the base-resin datasheet.
The grade should not be steam-sterilized at 121 °C; the polymer softens and undergoes creep under pressure at sterilization temperatures. It is not formulated for continuous outdoor exposure without UV stabilizer addition. Direct contact with aromatic hydrocarbons, chlorinated solvents, or strong oxidizing acids leads to swelling, stress cracking, or oxidative degradation; these environments are outside the intended packaging and stretch-film uses. The base resin contains only processing antioxidants, not long-term thermal stabilizers for underhood or hot-water service. When coextruded with polyamide or ethylene vinyl alcohol, an adhesive tie layer is required because interfacial incompatibility causes delamination at the molecular boundary. Pellets should be stored indoors and kept free of fine dust; contamination by even small amounts of high-molecular-weight polypropylene or high-density polyethylene can form visible gel-like defects in the cast melt curtain.