| HS Code | 214741 |
| Product | Dow DOWLEX™ 2517 Linear Low Density Polyethylene, Narrow MW Distribution |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | 1-Octene |
| Molecular Weight Distribution | Narrow |
| Density | 0.917 g/cm3 |
| Melt Index 190 C 2 16 Kg | 25 g/10 min |
| Tensile Strength At Yield | 8.7 MPa |
| Tensile Strength At Break | 10.3 MPa |
| Elongation At Break | 800% |
| Flexural Modulus | 193 MPa |
| Vicat Softening Point | 88°C |
| Melting Point | 122°C |
| Shore D Hardness | 50 |
| Notched Izod Impact Strength At 23 C | No Break |
As an accredited Dow DOWLEX™ 2517 Linear Low Density Polyethylene, Narrow MW Distribution factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Dow DOWLEX 2517 LLDPE is supplied in 25 kg multiwall bags, typically palletized for secure handling and storage. |
| Container Loading (20′ FCL) | Container loading 20′ FCL: palletized 25 kg bags of Dow DOWLEX™ 2517 LLDPE, narrow MW distribution, shrink-wrapped, secured for ocean transport. |
| Shipping | DOWLEX™ 2517 LLDPE is shipped as non-hazardous polyethylene pellets in 25 kg bags, 1,000 kg bulk bags, or bulk trucks/railcars. Store in a cool, dry, well-ventilated area, keeping containers closed and away from heat, sunlight, and ignition. Not DOT/IMDG regulated; no special hazard labels required. |
| Storage | For Dow DOWLEX™ 2517 Linear Low Density Polyethylene, Narrow MW Distribution, store in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, flames, and strong oxidizers. Keep bags/containers closed to prevent moisture, dust, and contamination. Use original packaging on stable pallets; avoid excessive stacking and static buildup. Maintain moderate temperatures, typically below 50°C, and follow local regulations. |
| Shelf Life | Shelf Life: Typically 24 months from manufacture when stored unopened in dry, cool conditions, away from direct sunlight and contamination. |
Dow DOWLEX™ 2517 Linear Low Density Polyethylene, Narrow MW Distribution is specified on the basis of a density of 0.917 g/cm³ determined under ASTM D792-20 and a melt index of 2.3 g/10 min at 190 °C/2.16 kg determined under ASTM D1238-20 or ISO 1133-1:2022. The narrow molecular weight distribution reduces the concentration of very high molecular-weight chains; this narrows shear-thinning response, supports low gel-related film defects, and creates a more defined melting range during blown film extrusion. The material is supplied as free-flowing pellets and can be processed on conventional polyolefin blown film lines without predrying when stored below 50% relative humidity; at higher humidity, hopper dryers are set to 60 °C for 2 h to remove surface moisture.
| Property | Method | Value |
|---|---|---|
| Density | ASTM D792-20 | 0.917 g/cm³ |
| Melt index | ASTM D1238-20 / ISO 1133-1:2022 | 2.3 g/10 min at 190 °C/2.16 kg |
| Peak melting point | ASTM D3418-21 | 122 °C |
On a three-layer coextrusion blown film line configured for fresh-cut vegetable pillow packs, the outer layers are run at 70 wt% to 80 wt% DOWLEX 2517 with 20 wt% to 30 wt% LDPE to stabilize the bubble at a die gap of 1.8 mm and a blow-up ratio of 2.2:1 to 2.8:1. The core layer may carry recycled trim at up to 15 wt% when the line is equipped with a screen changer and a gear pump sufficient to hold melt pressure variation below ±0.5 bar. Antiblock masterbatch is added at 0.5 wt% to 1.5 wt% and slip masterbatch at 0.5 wt% to 1.0 wt%; these levels are adjusted against a film coefficient of friction target of 0.20 to 0.30 measured under ASTM D1894-14 after 24 h of migratory conditioning. Compliance for direct food contact in pillow packs is evaluated under FDA 21 CFR 177.1520(c) and EU Regulation (EU) No 10/2011 Annex I and III; total migration testing is performed with simulant D2 or E according to the intended shelf life, with an overall migration limit of 10 mg/dm². Downstream conversion uses a 70 mm 30:1 L/D single-screw extruder for the outer layers, a 90 mm 30:1 L/D extruder for the core, a 400 mm die, dual-lip air ring cooling, and a post-nip corona treater set to 38–42 mN/m surface energy for flexographic printing. Terminal film thickness is 25 µm to 50 µm, slit into register-run bags for cut lettuce, spinach, and mixed salad formats.
A monolayer blown film line running 70 wt% DOWLEX 2517 and 30 wt% LDPE for IQF vegetable pouches is normally tested for low-temperature puncture at the seal fold rather than for tensile yield alone; the film is conditioned at −18 °C and evaluated under ASTM D1709-16a and ASTM D1922-15. The extrusion set-up uses a 55 mm 25:1 L/D barrier screw, a 350 mm spiral die, a die gap of 1.6–2.0 mm, a blow-up ratio of 2.5:1, and a frost line held at 600–800 mm above the die face. The narrow molecular weight distribution keeps gel count low enough for vertical form-fill-seal jaw cycling at 60–80 cycles/min, but bubble oscillation rises when the frost line is pushed beyond 900 mm or when melt temperature exceeds 235 °C; line operators report helical instability at the bubble shoulder, which transfers into gauge bands at the seal areas. Anti-fog masterbatch is added at 1.0–3.0 wt%, slip at 0.5–1.0 wt%, and antiblock at 0.5–1.5 wt%; anti-fog performance is assessed by hot fog measurement under ASTM D1003-21 after 48 h at 4 °C and 24 h at −18 °C. U.S. food contact compliance is under FDA 21 CFR 177.1520(c) with conditions of use appropriate to frozen and refrigerated filling; EU compliance requires EU Regulation (EU) No 10/2011 specific migration testing in 10% ethanol and 3% acetic acid simulants for the declared shelf period. Terminal packages include 1 kg frozen vegetable pouches, 500 g IQF seafood bags, and recloseable freezer carton liners. Published data for this specific VFFS configuration is limited, so the dart impact threshold is best established on the target line after jaw-speed and seal-bar pressure calibration.
Silage cover and greenhouse film lines typically run DOWLEX 2517 in a three-layer structure in which the core contains UV-stabilized trim and the skin layers are formulated from 100 parts DOWLEX 2517, 5–8 wt% UV masterbatch based on hindered amine light stabilizer chemistry, 1–2 wt% anti-fog masterbatch, and 0.5–1.5 wt% slip/antiblock. The die gap is 2.0 mm, the blow-up ratio is 2.5:1 to 3.0:1, and the melt temperature is held at 210–225 °C to limit crosslinking of the HALS package. Compliance is assessed under EN 13206:2017 for agricultural covering films, including mechanical retention after artificial weathering under ISO 4892-2:2013; for multi-season greenhouse applications, the film must retain at least 50% of initial tensile yield after 3,000 h exposure. Sulfur contact from greenhouse vaporization systems requires the use of NOR-HALS rather than standard HALS because sulfur dioxide deprotonates secondary amine light stabilizers and accelerates film surface crazing; this failure is reported on greenhouse flanks facing pesticide foggers. Downstream conversion uses a 75 mm 30:1 L/D extruder with a 500 mm annular die and internal bubble cooling; the lay-flat width is set to 1.2–2.0 m and roll length to 2,000 m for export palletization. Terminal products include silage pit covers, greenhouse cladding, and strawberry tunnel film in thicknesses from 80 µm to 150 µm.
At 60 wt% loading in a heavy-duty shipping sack film, the remainder is split between 20 wt% LDPE for bubble stability and 20 wt% internally recycled edge trim, provided the reclaimed fraction is screened through a 100 µm melt filter to remove char and oxidized gel. The formulation target is a film with secant modulus at 1% elongation of 140–180 MPa in the machine direction measured under ASTM D882-18 and an Elmendorf tear strength exceeding 25 N/mm in the cross direction measured under ASTM D1922-15. The line uses a 90 mm 30:1 L/D single-screw extruder running at 80 kg/h on a 500 mm die with 2.2 mm die gap, a blow-up ratio of 2.0:1 to 2.5:1, and a melt temperature of 215–230 °C; lower melt temperatures are avoided because the narrow MWD resin increases screw torque and die pressure more rapidly than a broad-MWD LLDPE of the same melt index. Compliance for industrial non-food sacks falls under REACH Regulation (EC) No 1907/2006, RoHS Directive 2011/65/EU for heavy metals, and Directive 94/62/EC for packaging and packaging waste where export to EU member states occurs. Downstream production includes flat-bed sealing at 120–140 °C and gusseted tubing collapse into valve sacks with a fill weight of 10–25 kg. Terminal products are heavy-duty sacks for polymer resin, carbon black masterbatch, and mineral filler shipments.
Pallet unitization stretch hood lines running three-layer coextrusion specify DOWLEX 2517 in the core at 70–85 wt%, with 10–20 wt% polyolefin elastomer and 5–10 wt% metallocene LLDPE for puncture resistance. The cling layer on one surface incorporates 1–3 wt% of a polymer modifier such as polyisobutylene, and the opposite surface contains 0.5–1.5 wt% antiblock to prevent blocking during roll storage. Film is extruded at 230–245 °C through a 500 mm spiral die with 2.0 mm die gap and oriented in the machine direction after reheating to 90–110 °C; the stretch ratio is limited to 1.5:1 to 2.0:1 to avoid draw resonance. Tensile properties are tested under ISO 527-3:2018, puncture resistance under ASTM D5748-19, and cling under ASTM D5458-95. The product does not involve food contact, but it must comply with REACH Regulation (EC) No 1907/2006 and the CLP Regulation; automotive or appliance supply chain exports may require IMDS entry and RoHS Directive 2011/65/EU compliance. Terminal products include 80–120 µm stretch hood films for palletized appliances, building material bundles, and automated high-speed pallet wrapping cells.
Competitive Dow DOWLEX™ 2517 Linear Low Density Polyethylene, Narrow MW Distribution prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
DOWLEX™ 2517 Linear Low Density Polyethylene, Narrow MW Distribution, is a high-flow ethylene/α-olefin copolymer produced by solution polymerisation. The grade is specified by a melt index of 25 g/10 min determined at 190 °C under a 2.16 kg load in accordance with ASTM D1238 and ISO 1133-1, and by a density of 0.917 g/cm³ determined in accordance with ASTM D792 or ISO 1183-1. The combination of low density, high melt index, and deliberately narrowed molecular weight distribution places this grade in the injection molding segment of the DOWLEX family, where it is used for thin-wall containers, closures, housewares, and multi-cavity packaging components. The narrow molecular weight distribution is the controlling architectural feature that differentiates the melt-phase elastic response, shear viscosity, mold shrinkage anisotropy, and frozen-in orientation from conventional broad-molecular-weight linear low density polyethylene grades.
In broad-MWD LLDPE, the high-molecular-weight tail contributes disproportionately to melt elasticity, recoverable shear strain, die swell, and relaxation time. These chains do not govern the melt index, which is measured at low shear rates, but they do influence filling behavior and dimensional stability in injection molding. In DOWLEX™ 2517, the reduction of this tail produces a melt that is less shear-thinning than a broad-MWD grade of identical 25 g/10 min melt index. Capillary rheometry in accordance with ASTM D3835 therefore records a viscosity at processing shear rates above 1,000 s⁻¹ that remains proportionally closer to the low-shear viscosity than would be observed in a broad-MWD control. The practical consequence is that single-point melt index overestimates the ease of filling under thin-wall conditions; mold-filling simulation should use actual viscosity curves rather than nominal melt flow ratings.
Because high-molecular-weight chains relax slowly, broad-MWD grades carry more molecular orientation from the gate into the cavity. That orientation generates anisotropic shrinkage after ejection, with the machine direction typically shrinking more than the transverse direction. With DOWLEX™ 2517, the narrower distribution shortens the longest relaxation times and lowers recoverable shear strain. Molded slabs and plaques show more uniform shrinkage when measured according to ISO 294-4 or ASTM D955, and warpage of flat lids is correspondingly reduced. The trade-off is that the same narrow distribution lowers melt strength in extensional flows; the grade is therefore not specified for blown film, blow molding, or extrusion foaming where bubble or parison stability requires strain hardening.
On reciprocating-screw injection molding machines, barrel set-points are selected to keep the melt temperature between 190 °C and 240 °C. Below 190 °C, solid-bed breakup in the compression zone is incomplete on general purpose screws with 20:1 to 24:1 L/D ratios, and the risk of cold slug formation, short shots, and excessive clamp force rises in thin-wall tools. Above 250 °C, oxidative chain scission accelerates, producing viscosity loss, surface bloom, and acrid odour in the melt pool; prolonged hold at this upper boundary should be avoided unless the barrel is purged frequently.
Mold temperatures between 10 °C and 40 °C are typical for thin-wall packaging. Turbulent-flow chilled water at 8 °C to 12 °C is used when cycle time is controlled by conduction through the frozen skin. At mold temperatures below 5 °C, condensation on cavity surfaces can occur under plant relative humidity above 60 %, producing splay that is unrelated to resin moisture. The resin is not hygroscopic, and drying is not required for hydrolysis control; however, pellets stored at temperatures below the injection plant dew point can carry surface moisture into the feed throat. When this occurs, a desiccant hopper set at 60 °C to 80 °C with a dew point of -20 °C or lower is sufficient to remove surface condensation before plastication.
For multi-cavity tools with valve-gated hot runners, the valve pin itself should not be operated below 220 °C because this grade has low melt elasticity and any cold skin at the gate can tear during pin retraction, generating stringing or gate pockmarks. Back pressure in the range of 0.5 MPa to 1.5 MPa is usually sufficient to homogenize the narrow-MWD melt without excessive shear heating; higher back pressure does not compensate for low barrel set-points and can extend recovery time.
For compounding or masterbatch dilution, the high melt index permits rapid wetting of pigments and fillers, but the narrow molecular weight distribution reduces viscous drag during distributive mixing. Single-screw compounders should use pegged or pineapple mixing sections rather than high-compression barrier screws intended for polyolefin film extrusion. Twin-screw extruders with 32:1 to 44:1 L/D ratios and downstream side feed are preferred for highly filled formulations because they limit residence time and prevent local melt temperatures from exceeding 250 °C.
Table 1 compiles representative physical property values published for DOWLEX™ 2517. These values are typical injection molded specimen data and are not to be read as contract specification limits; individual certificates of analysis govern each lot.
| Property | Test method | Typical value |
|---|---|---|
| Melt index | ASTM D1238 / ISO 1133-1 | 25 g/10 min |
| Density | ASTM D792 / ISO 1183-1 | 0.917 g/cm³ |
| Tensile strength at yield | ASTM D638 / ISO 527-2 | 10 MPa |
| Tensile elongation at break | ASTM D638 / ISO 527-2 | 800 % |
| Flexural modulus, 1% secant | ASTM D790 / ISO 178 | 220 MPa |
| Vicat softening temperature | ASTM D1525 / ISO 306 | 88 °C |
| Melting temperature, DSC | ASTM D3418 | 121 °C |
| Hardness | ASTM D2240 / ISO 868 | 51 Shore D |
The 0.917 g/cm³ density and 25 g/10 min melt index are the two specification-critical values most commonly controlled during lot release. Because the grade is produced with a narrow molecular weight distribution and low long-chain branching, density correlates differently with stiffness than in high-pressure LDPE: the short-chain branch content lowers crystallinity and secant modulus while retaining ductility and low-temperature flexibility. Mechanical property values in Table 1 should be used only for material preselection; finished part performance must be validated on the actual tool because cooling rate, gate geometry, and orientation control the solid-state morphology.
The first measurable difference appears in the filling phase of injection molding. Because narrow-MWD LLDPE is less shear-thinning, the pressure required to fill a given tool is not automatically reduced by the 25 g/10 min rating. Where a broad-MWD grade of identical melt index may drop to a lower viscosity at gate shear rates, DOWLEX™ 2517 retains a higher viscosity at equivalent shear rate. The difference should be quantified by mold-filling simulation or by in-mold pressure transducers, not by melt index alone. The compensating benefit is lower elastic turbulence at the gate, lower jetting tendency, and more uniform molecular orientation in the frozen layer.
After ejection, the narrow-MWD part typically exhibits lower warpage and less machine-direction/transverse-direction shrinkage differential. Shrinkage measurements carried out in accordance with ASTM D955 on 2 mm plaques differentiate the grade from broad-MWD LLDPE because the high-molecular-weight tail is the main source of slow, post-ejection relaxation. The residual stress profile through the thickness is therefore less asymmetric. In applications such as flat lids or shallow trays, this property reduces dimensional scrap rates. Conversely, the same architectural feature lowers melt strength, so the grade should not be transferred to blow molding or deep-draw thermoforming without direct evaluation.
Compared with high-pressure LDPE of similar density and melt index, DOWLEX™ 2517 has higher tensile yield strength and puncture resistance because the linear ethylene backbone with short-chain branches produces tighter tie-chain networks at equal crystallinity. Instrumented puncture testing in accordance with ASTM D3763 and tensile testing in accordance with ASTM D638 demonstrate this difference, although high melt index reduces ultimate elongation relative to fractional-melt-index LLDPE. The high-pressure LDPE grade retains higher extensional viscosity and is better suited to extrusion coating and blown film; the present grade is narrower in molecular weight distribution and is therefore optimized for injection molding rather than melt-extension processes.
Within the DOWLEX range, the main differentiating variable is melt index. Film grades such as DOWLEX™ 2045 have a melt index in the order of 1 g/10 min and are designed for bubble stability and film toughness; DOWLEX™ 2517 is approximately 25 times higher in melt flow and is mobile enough for thin-wall filling but has shorter chain length and lower toughness. This is not a defect but a conversion route optimization. For applications requiring aggressive environmental stress crack resistance, a lower-melt-index LLDPE or a medium-density polyethylene selected for ASTM D1693 condition A testing is often preferred if the wall section and flow length allow the lower melt flow.
Lot-to-lot release documentation typically covers melt index, density, and visual pellet contamination. Regulatory suitability for food-contact use is assessed under FDA 21 CFR 177.1520 for olefin polymers; compliance is end-use specific, and migration testing on the finished article is required for fatty food simulants under US FDA conditions of use and for overall migration under Commission Regulation (EU) No 10/2011 using EN 1186-1. For European food-contact compliance, specific migration limits for comonomer-derived oligomeric species may be measured by methods in the EN 13130 series. The grade contains no intentionally added heavy metals above the concentration limits in Directive 2011/65/EU (RoHS recast) for polyolefin packaging applications, and is subject to REACH registration obligations at the supplier level. None of these statements substitutes for the certificate of analysis or the supplier’s product regulatory bulletin.
| Requirement | Standard or regulation | Measurement or scope |
|---|---|---|
| Melt index control | ASTM D1238 / ISO 1133-1 | 25 g/10 min at 190 °C / 2.16 kg |
| Density control | ASTM D792 / ISO 1183-1 | 0.917 g/cm³ |
| U.S. food-contact status | FDA 21 CFR 177.1520 | Olefin polymers; end-use migration testing required |
| EU food-contact status | Commission Regulation (EU) No 10/2011 | Overall migration by EN 1186-1; specific migration limits apply |
| RoHS recast | Directive 2011/65/EU | No intentionally added Pb, Cd, Hg, Cr(VI), PBB, PBDE above limits |
In production-scale molding, the most common failure mode with this narrow-MWD grade is not melt degradation but gate-stringing from low melt elasticity. When the hot-runner gate is cooled too aggressively, the valve pin tears a frozen skin from the cavity. Processing observations from multi-cavity packaging tools indicate that the nozzle and hot runner are often run 5 °C to 10 °C above the barrel mid-range, not primarily to reduce viscosity but to keep the gate skin soft enough for clean separation. If stringing persists, reducing mold temperature is usually less effective than increasing gate orifice temperature. The grade should also be protected from extended residence time at melt temperature above 250 °C, and purging with a general-purpose LDPE at 200 °C to 230 °C is recommended when transitioning from high-temperature engineering resins.