| HS Code | 747564 |
| Grade Name | DOWLEX™ 2267G |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | 1-Octene |
| Density | 0.917 g/cm³ |
| Melt Index 190 C 2 16 Kg | 2.3 g/10 min |
| Melt Flow Ratio I10 I2 | 8.0 |
| Melting Point | 122 °C |
| Vicat Softening Point | 94 °C |
| Tensile Strength At Yield | 10.3 MPa |
| Tensile Strength At Break | 28.3 MPa |
| Elongation At Break | 800% |
| Flexural Modulus | 240 MPa |
| Dart Impact Strength | 200 g |
| Elmendorf Tear Strength Md | 250 g |
| Elmendorf Tear Strength Td | 350 g |
| Haze | 10% |
| Gloss 45 | 60 |
| Coefficient Of Friction | 0.2 |
As an accredited Dow DOWLEX™ 2267G Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Dow DOWLEX™ 2267G LLDPE typically comes in 25 kg polyethylene-lined paper bags, palletized and shrink-wrapped for industrial use. |
| Container Loading (20′ FCL) | 20′ FCL: DOWLEX™ 2267G LLDPE in 25 kg bags, palletized, stretch-wrapped, forklift-loaded; approximately 24–25 MT per dry container. |
| Shipping | Dow DOWLEX™ 2267G Linear Low Density Polyethylene is shipped as non-hazardous solid resin pellets. Standard packaging includes 25 kg bags on pallets, supersacks, or bulk trucks/railcars. Keep containers closed, dry, and away from heat or ignition. Follow local regulations and the supplier’s SDS. |
| Storage | Store DOWLEX™ 2267G in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, flames, and strong oxidizers. Keep containers/packages closed and labeled. Prevent dust accumulation and moisture exposure. Use appropriate grounding if handling bulk. Maintain ambient temperature, avoid excessive stacking, and follow supplier SDS and local regulations. Do not store near food, drink, or incompatible materials. |
| Shelf Life | Under recommended cool, dry storage, Dow DOWLEX™ 2267G typically has a shelf life of two years in unopened packaging. |
On 5-layer cast film lines equipped with 80/100/70 mm barrier-screw extruders, a 2500 mm automatic die, and vacuum-box edge pinning, DOWLEX 2267G is metered into the core and back-side skin layers at 70–85 wt%. The extrusion profile from feed throat to adapter is typically set at 175 °C, 200 °C, 220 °C, 240 °C, and 260 °C, with melt temperature at the die held between 245 °C and 270 °C as measured by infrared probe. A die gap of 0.5–0.8 mm, air gap of 90–150 mm, chill roll surface temperature of 18–28 °C, and line speed of 300–650 m/min are used to fix web gauge while limiting crystallinity loss in the outer skin. The compound comprises 10–20 wt% high-pressure LDPE for draw stability, 1–3 wt% polyisobutylene cling masterbatch in the cling skin, 0.05–0.15 wt% hindered phenolic antioxidant, and 5000–10000 ppm silica antiblock in the reverse skin. Gauge profiling across the web is controlled through 10–20 µm automatic die-bolt adjustment zones, and corona treatment is held at 38–42 dyn/cm before winding. Quality verification uses ISO 527-3:2018 for tensile yield, ASTM D5748-14(2019) for puncture-propagation resistance, and ASTM D5459-14 for machine-direction elastic recovery and stress retention. The resulting pallet overwrap is produced at 12–35 µm thickness and is validated for stretched elongation from 150% to 250% on automatic rotary-ring and turntable wrappers. Regulatory compliance is assessed under FDA 21 CFR 177.1520(c) 3.2a for olefin polymers, EU Regulation (EU) No 10/2011 with an overall migration limit of 10 mg/dm² in assigned food simulants, and REACH Regulation (EC) No 1907/2006. When the film is used in electrical or electronic product packaging, RoHS Directive 2011/65/EU homogeneous-material limits of 1000 mg/kg lead, 1000 mg/kg mercury, 1000 mg/kg hexavalent chromium, 1000 mg/kg PBB/PBDE, and 100 mg/kg cadmium must be met by the finished article.
| Domain | Reference | Scope | Limit or test method |
|---|---|---|---|
| United States food contact | FDA 21 CFR 177.1520(c) 3.2a | Olefin polymers used in contact with food | Extraction limits assigned by food type and use condition |
| European food contact | EU Regulation (EU) No 10/2011 | Plastic materials and articles intended for food contact | Overall migration 10 mg/dm²; specific migration limits per Annex II |
| Chemical registration | REACH Regulation (EC) No 1907/2006 | Article and substance obligations | SVHC communication threshold 0.1 wt% |
| Electrical and electronic packaging | RoHS Directive 2011/65/EU | Homogeneous material restrictions | Lead 1000 mg/kg; cadmium 100 mg/kg; mercury 1000 mg/kg; Cr(VI) 1000 mg/kg |
| Packaging waste | EU Packaging Directive 94/62/EC | Heavy metals in packaging | Sum of lead, cadmium, mercury, Cr(VI) 100 mg/kg by weight |
Blending DOWLEX 2267G into heavy-duty blown-film sack layers at 20–40 wt% raises low-temperature puncture resistance but shifts the melt-strength balance on conventional low-pressure long-stalk extrusion lines. The process configuration uses 1.2–1.6 mm die gaps, die temperature of 200–215 °C, blow-up ratio of 2.2:1–2.6:1, and frost-line height maintained at 8–12 die diameters. Bubble instability is observed when the blow-up ratio exceeds 2.8:1 or when the high-pressure LDPE content falls below 50 wt%, because the resulting melt strength is insufficient to resist helical instabilities on air-ring-cooled bubbles. The sack layer compound is composed of 20–40 wt% DOWLEX 2267G, 60–80 wt% high-pressure LDPE, 2–4 wt% grey or blue masterbatch, and 200–500 ppm fluoropolymer processing aid. The final three-ply gusseted sack is produced on a tandem blown-film line with 500–1200 kg/h output capacity and automatic surface winding. Dart impact is measured according to ASTM D1709-16a, Elmendorf tear according to ASTM D1922-15, and tensile properties according to ISO 527-3:2018. Heavy-duty sack applications require a falling-dart impact of 600–1200 g on 150–200 µm film, depending on fill weight and drop-cycle severity. Food-contact grades for paper-plastic and film liner sacks follow FDA 21 CFR 177.1520(c) 3.2a; non-food industrial liners are qualified under REACH Regulation (EC) No 1907/2006. Processing with reclaimed in-plant scrap above 30 wt% without a melt screen pack rated at 80–120 µm can increase gel counts and reduce dart-impact reproducibility, though published production data for this specific grade in high-recyclate sack structures is limited.
Three-layer silage and greenhouse films require a different molecular-weight distribution in the skin layers than in the barrier core, and DOWLEX 2267G is used in the skins at 60–70 wt% with 20–30 wt% LDPE, 3–6 wt% UV stabilizer masterbatch, 0.5–1.5 wt% tackifier, and 0.05–0.2 wt% zinc stearate. The blown-film process runs at a melt temperature of 205–225 °C, die gap of 1.4–1.8 mm, blow-up ratio of 2.0:1–2.5:1, and an elevated frost line to reduce film haziness. The coextruded structure places a polyamide or EVOH core between two DOWLEX 2267G-based skins to limit oxygen ingress during ensiling. Film thickness in silage wrap ranges from 25 µm to 45 µm; greenhouse cover films are produced at 150–200 µm. Tensile and tear properties are verified by ISO 527-3:2018 and ISO 6383-2. For agricultural use, food-contact migration rules do not apply unless the film is intended for direct contact with feed; otherwise, REACH Regulation (EC) No 1907/2006 and EU Regulation (EU) No 10/2011 are evaluated only where the silage film is used adjacent to feed-contact laminates. UV stabilizer packages should be matched to the specific HALS and benzotriazole chemistry recommended by the masterbatch supplier; overdosing transition-metal stearates in combination with anti-acid scavengers can accelerate oxidative degradation and reduce film life below the expected 12–24 month outdoor exposure window.
Extrusion coating lines for liquid packaging board blend DOWLEX 2267G with high-pressure LDPE at 15–30 wt% in the 15–25 µm coating layer to reduce neck-in while preserving heat-seal response through a downstream flame or corona treatment. The extrusion coating process runs a 90 mm extruder with a barrier screw and 300 mm flat die, melt temperature of 285–310 °C, die gap of 0.5–0.7 mm, air gap of 150–250 mm, and chill roll surface temperature of 15–20 °C at line speeds from 250 m/min to 400 m/min. Corona pre-treatment is set at 40–44 dyn/cm and ozone dosing is held at 2–4 g/h to raise adhesion to the paperboard substrate without excessive oxidation of the polyethylene surface. The polymer layer is required to pass seal-strength testing under ASTM F88/F88M-23 after jaw sealing at 120–150 °C and 300–500 N sealing force. The finished beverage carton laminate is evaluated under FDA 21 CFR 177.1520(c) 3.2a and EU Regulation (EU) No 10/2011, with an overall migration limit of 10 mg/dm²; for fatty liquid simulants, the assigned simulant D2 under EU Regulation (EU) No 10/2011 is used. Processing boundaries are defined by oxidative degradation: melt temperature above 320 °C increases gel formation and off-odor, and a nitrogen blanket on the feed hopper is required when line downtime exceeds 15 min at temperature. The resin is not recommended as the sole extrusion-coating polymer because its melt draw characteristics are not equivalent to dedicated autoclave LDPE, and polymer blends exceeding 50 wt% DOWLEX 2267G tend to increase edge-bead thickness and require more aggressive edge-trim recycling.
Post-consumer recyclate streams containing 60–80 wt% LLDPE film scrap are compounded with DOWLEX 2267G at 20–40 wt% to restore tear resistance and seal integrity in refuse sacks and industrial can liners. Compounding is performed on a 60 mm twin-screw extruder with L/D 40:1, vacuum venting at 150–200 mbar, melt temperature of 210–230 °C, and an underwater die-face pelletizer. The formulation includes 0.1–0.2 wt% hindered phenolic/phosphite antioxidant and 200–400 ppm fluoropolymer processing aid; the melt-filtration screen pack uses 100–150 µm mesh to remove non-melting contaminants from post-consumer film. Recyclate streams contaminated with polypropylene above 5 wt% reduce dart impact and can produce layer delamination in the finished sack, so density-based sorting before pelletizing is required. Finished film properties are checked under ASTM D638-14 for tensile yield and break, ASTM D1709-16a for falling-dart impact, and ISO 1133-1:2022 for lot-to-lot melt-flow stability. Regulatory qualification is limited to non-food applications; REACH Regulation (EC) No 1907/2006 applies to the recyclate fraction, and the finished packaging must satisfy the EU Packaging Directive 94/62/EC sum limit of 100 mg/kg for lead, cadmium, mercury, and hexavalent chromium. Published data for DOWLEX 2267G in highly contaminated post-consumer PP-limited streams is limited, so pilot-scale extrusion and gel-count analysis are required before plant-wide deployment.
Competitive Dow DOWLEX™ 2267G Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Dow DOWLEX™ 2267G Linear Low Density Polyethylene is a solution-polymerized ethylene-octene copolymer supplied as pellets for cast film extrusion. The resin is identified by a nominal density of 0.917 g/cm³ measured under ASTM D792-20 and a melt index of 2.3 g/10 min at 190°C and 2.16 kg load according to ASTM D1238-20. These two values are the primary incoming raw-material controls; density is determined by gradient column or displacement pycnometry, while melt index is measured in a dead-weight plastometer with a 2.095 mm die orifice and 8.0 mm bore. The grade is intended for cast film in industrial stretch wrap, where downgauging and high pre-stretch are production requirements. This usage differs from typical blown-film DOWLEX grades because the melt-index placement of 2.3 g/10 min is higher than extrusion-coating or heavy-duty sack grades, reducing melt pressure and enabling thinner die gaps. Published supplier documentation also links the resin to surface protection film and food-packaging laminates when converted under appropriate film-forming conditions. The additive package may include slip and antiblock at loadings that are not specified in the general datasheet; the certificate of analysis should be consulted for lot-level values.
Thermal properties obtained from differential scanning calorimetry in accordance with ISO 11357-3:2018 include a peak melting point of approximately 122°C, while Vicat softening point is commonly reported between 96°C and 98°C under ASTM D1525-17e1 with a 10 N load. These thermal values are not processing setpoints; they indicate the crystalline melting range that defines the lower melt-temperature boundary for cast film operation.
Incoming resin handling requires silo or Gaylord management. Pellets should be conveyed with filtered, dried air at 30–40°C to avoid surface condensation; bulk-silo residence time above 72 h at ambient humidity greater than 60% can produce the same splay defects observed in film below 20 µm. On production casting lines with 90 mm extruders, the resin is frequently run with a screen pack of 40/60/80 mesh and a breaker plate pressure transducer; the pressure drop across the screen pack should not exceed 80 bar during steady operation.
In DOWLEX 2267G, the use of 1-octene as comonomer introduces short-chain branches of six carbon atoms along the ethylene backbone. The branches disrupt polyethylene crystallinity more effectively than the ethyl branches formed from 1-butene at equivalent comonomer content, so the density is reduced to 0.917 g/cm³ and the crystalline fraction is lower than that of butene-based LLDPE of similar melt index. The amorphous phase contains tie molecules that connect adjacent lamellae; under rapid deformation, these tie molecules redistribute stress before chain scission. This morphology is reflected in film tests such as dart impact per ASTM D1709-16a, Elmendorf tear per ASTM D1922-15, and puncture resistance per ASTM D5748-19. Published data for 25 µm cast film produced from DOWLEX 2267G are configuration-dependent; variation in die gap, draw ratio, and chill roll temperature can shift tear balance by more than 20%.
The narrow molecular weight distribution associated with the solution polymerization process differs from the broad distribution of high-pressure LDPE. This molecular architecture reduces shear sensitivity and yields more predictable laminar flow through coat-hanger dies; however, it also lowers melt strength relative to LDPE. Consequently, DOWLEX 2267G is positioned for cast film rather than shrink film or blown film requiring high bubble stability.
Tear balance can be altered by die gap and draw ratio. A die gap of 0.75 mm and a draw ratio of 20:1 may produce machine-direction tear below 2.0 N in 25 µm film, while transverse-direction tear may exceed 4.0 N; these values are not specifications but are representative of the anisotropic morphology created by uniaxial orientation on cast film lines.
| Grade or reference class | Nominal density | Melt index | Comonomer type | Primary conversion route |
|---|---|---|---|---|
| DOWLEX 2267G | 0.917 g/cm³ | 2.3 g/10 min | 1-octene | Cast film |
| DOWLEX 2045G | 0.920 g/cm³ | 1.0 g/10 min | 1-octene | Blown film |
| Conventional C4-LLDPE reference | 0.918–0.920 g/cm³ | 0.8–1.2 g/10 min | 1-butene | Blown or cast film, general purpose |
Distinctions from high-pressure low-density polyethylene are measurable by extensional rheology. In Rheotens testing with a capillary rheometer and drawing unit operating at 190°C, LDPE grades with long-chain branching exhibit pronounced strain-hardening and extensional viscosity growth above a draw ratio of 10:1; DOWLEX 2267G, having a predominantly linear backbone with octene short branches, shows lower strain-hardening intensity. That molecular difference makes the resin suitable for high draw-down cast film lines using 0.6–1.0 mm die gaps, but it limits the use of the grade in thick blown film where bubble support depends on melt stiffness. In cast film, the absence of high-pressure LDPE long-chain branching also reduces melt fracture at high output rates, provided the die is maintained at 230°C or above.
Compared with metallocene-catalysed plastomers of density 0.900–0.910 g/cm³, DOWLEX 2267G retains a higher crystalline melting point near 122°C and higher stiffness, measured as flexural modulus. That places the resin between conventional butene LLDPE and true plastomers in the stiffness–puncture continuum.
Conversion of DOWLEX 2267G on cast film lines generally uses single-screw extruders with an L/D ratio of 24:1 to 30:1 and a barrier screw with a Maddock mixing section. Pebble or smooth-bore feed sections are both encountered; grooved-feed extruders require careful temperature control in the feed throat below 50°C to avoid pellet bridging. With the melt index of 2.3 g/10 min, head pressure at a 90 mm extruder running at 80 min⁻¹ is typically in the range of 150–250 bar; pressures above 300 bar indicate screen pack blockage or insufficient heating. Start-up melt temperature should be set between 230°C and 260°C at the die, with lower settings for high-gloss film and higher settings for low-haze orientation.
Chill roll temperature is a critical variable. In cast film manufacture, chill roll surface temperatures between 15°C and 30°C are used to set the quench rate; at temperatures above 35°C, haze measured by ASTM D1003-13 may increase because slower crystallization produces larger spherulites. The air gap between die exit and chill roll is normally 10–20 cm. Longer air gaps increase film neck-in and edge trim losses; shorter air gaps can cause draw resonance in film below 15 µm.
Moisture-related defects are uncommon in LLDPE, but pellets stored at relative humidity above 60% should be protected from surface condensation. Splay, die lines, and thickness variation in films below 20 µm have been observed when cold resin is transferred directly into a warm feed throat without a purge transition of at least 30 minutes.
Food-contact status is established by the final article, not by the resin alone. DOWLEX 2267G is generally covered under 21 CFR 177.1520(c)(3.2a) for olefin polymers intended for contact with food, provided the polymer meets density and melt-flow criteria and the finished package complies with applicable extractives limitations. Under European obligations, compliance is assessed according to Commission Regulation (EU) No 10/2011 and its amendments, including the overall migration limit of 10 mg/dm² and specific migration limits listed in Annex I; migration testing methods are specified in the EN 1186 series.
For REACH, polymers are exempt from registration under EC No 1907/2006, but monomer and additive substances must be registered; the grade may be sold only after the corresponding monomers and additives are registered for the appropriate tonnage band. A supplier declaration for substances of very high concern should be requested for each lot in accordance with REACH Article 33.
| Regulatory area | Identifier or test method | Applicability to DOWLEX 2267G |
|---|---|---|
| U.S. food contact | 21 CFR 177.1520(c)(3.2a) | Coverage as an olefin polymer; final article extractives apply |
| EU food contact | (EU) No 10/2011, EN 1186 | Overall migration limit 10 mg/dm²; additive-specific migration limits apply |
| REACH | EC No 1907/2006 | Polymer exemption; monomers and additives registered; SVHC communication required |
RoHS Directive 2011/65/EU restrictions do not directly govern food-packaging film unless components are incorporated into electrical and electronic equipment; lead, cadmium, mercury, hexavalent chromium, and PBB/PBDE concentrations in the resin should still be confirmed by supplier documentation for downstream compliance.
Downgauging below 12 µm transfers stress from bulk yielding to surface and interfacial failure mechanisms. For high-speed pallet wrappers using pre-stretch ratios of 200% to 300%, the film is elongated between rollers before wrapping; machine-direction tensile strength is typically specified in the range of 25–35 MPa according to ASTM D882-18, but published data for DOWLEX 2267G at 10 µm are limited and should be generated on the target wrapper rather than extrapolated from 25 µm laboratory film.
Puncture resistance under ASTM D5748-19 is a more direct predictor of pallet-load security than tensile yield, especially where irregular loads create point contacts. Octene-based LLDPE grades with density near 0.917 g/cm³ are selected because lower crystalline yield strength allows local deformation without catastrophic fracture; this behavior is different from high-density polyethylene and from butene-based LLDPE at the same film thickness.
Coefficient of friction should be measured after 40 h aging at 23°C ± 2°C per ASTM D1894-14 because surface slip additives migrate over time. Films intended for pre-stretch wrapping frequently require a kinetic coefficient of friction below 0.30, but targets vary with wrapper brand and film tension. Storage of finished rolls above 30°C can increase blocking force measured by ASTM D3354-15, particularly on the outer layers of large-diameter rolls.
At pre-stretch ratios above 250%, the film enters the strain-hardening region; if the resin has undergone excessive orientation, tear propagation in the machine direction can rise sharply. Converters often measure stretch force at 200% elongation using a force-strain tester; target values are line-specific but generally fall between 10 N and 20 N for 20 µm cast stretch film.
Operational boundary: If additional slip is dry-blended at the converter, loadings above 1000 ppm erucamide may cause plate-out on chill rolls and unstable film tension; dosing should be evaluated in a masterbatch carrier rather than added as neat powder.