| HS Code | 622920 |
| Density | 0.922 g/cm³ |
| Melt Index 190 C 2 16 Kg | 2.3 g/10 min |
| Melting Point | 124 °C |
| Vicat Softening Point | 104 °C |
| Tensile Strength At Yield Md | 11 MPa |
| Tensile Strength At Yield Td | 11 MPa |
| Tensile Strength At Break Md | 32 MPa |
| Tensile Strength At Break Td | 28 MPa |
| Elongation At Break Md | 600% |
| Elongation At Break Td | 700% |
| Elmendorf Tear Strength Md | 200 g |
| Elmendorf Tear Strength Td | 400 g |
| Dart Drop Impact | 120 g |
| Haze | 14% |
| Gloss 45 | 60% |
| Coefficient Of Friction | 0.2 |
As an accredited Dow DOWLEX™ 2267A Linear Low Density Polyethylene, Blown Film Grade factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg polyethylene-lined multiwall paper bags, palletized and stretch-wrapped; also available in 1,000 kg bulk bags. |
| Container Loading (20′ FCL) | 20′ FCL: approximately 18–20 MT of DOWLEX™ 2267A in 25 kg bags, palletized or floor-loaded, shrink-wrapped, and securely braced for ocean transport. |
| Shipping | Dow DOWLEX™ 2267A is typically supplied in 25 kg polyethylene bags, palletized and stretch-wrapped. Ship in clean, dry trucks or containers at ambient temperature. Protect from moisture, direct sunlight, and contamination; avoid punctures. Not classified as dangerous goods for transport. Handle per SDS and local regulations. |
| Storage | Store DOWLEX™ 2267A in a cool, dry, well-ventilated area at ambient temperature. Keep original bags or containers closed, palletized, and off the floor. Protect from direct sunlight, heat, ignition sources, moisture, and contamination. Avoid contact with oxidizers, acids, and bases. Use first-in, first-out stock rotation. Maintain clean handling to minimize dust and static buildup, and provide spill containment. |
| Shelf Life | No fixed shelf life; store in a cool, dry, well-ventilated area away from heat, sunlight, and moisture in original packaging. |
When DOWLEX 2267A is fed as the primary resin in heavy-gauge industrial sack film, extrusion is normally configured with a 1.6–2.4 mm die gap and a blow-up ratio of 2.2:1–3.0:1 to balance machine-direction and transverse-direction tear propagation. The resin carries a supplier-listed density of 0.917 g/cm³ and a melt flow rate of 2.3 g/10 min under ASTM D1238 at 190°C with 2.16 kg. For fertiliser, mineral, polymer pellet, and aggregate sacks at 120–180 µm, the film is generally a three-layer coextrusion with an HDPE-rich outer skin for stiffness and a DOWLEX 2267A-rich core for puncture, tear, and seal integrity. Melt temperatures of 210–240°C at the die and backpressure of 180–320 bar on 24:1 to 30:1 single-screw lines are typical. A silica antiblock loading of 2000–5000 ppm and an erucamide slip level of 300–1000 ppm are controlled to hold coefficient of friction between 0.20 and 0.35 under ASTM D1894; slip above 1000 ppm can reduce side-seal strength below 25 N/15 mm on 150 µm film when measured under ASTM F88. Dart drop impact is commonly specified at a minimum of 120 g under ASTM D1709 Method A, and transverse-direction Elmendorf tear is specified at or above 150 g under ASTM D1922 for 150 µm gauge products, although published data for this specific configuration is limited. Industrial sack compliance turns on REACH and RoHS 2011/65/EU thresholds, with lead below 0.1 wt% and cadmium below 0.01 wt% in homogeneous material. Where food-contact sacks are required, the resin is assessed under FDA 21 CFR 177.1520 olefin polymer clearance and EU 10/2011 overall migration limits.
Antiblock addition in frozen food webs does not produce a linear loss in clarity; the particle size distribution and refractive index of the selected silica, not loading alone, control haze development. For 50–80 µm films used in direct-contact packaging of frozen vegetables, fish, and dough, DOWLEX 2267A is blended with 10–20 wt% LDPE to improve bubble stability at elevated frost-line height, while slip and antiblock masterbatches are dosed to achieve 1500–4000 ppm silica and 400–1000 ppm erucamide. Haze under ASTM D1003 is typically specified below 8% on 50 µm film, and 60° gloss under ASTM D2457 is specified above 70; erucamide migration over 24–72 h can reduce coefficient of friction from 0.50 to 0.20 under ASTM D1894, so online corona treatment is scheduled before lamination or printing to avoid surface energy decay below 38 mN/m. Cold-crack resistance is not inferred from density alone; film is tested under ASTM D746 after conditioning at -30°C, and webs with higher dart drop impact under ASTM D1709 Method A are selected because low-temperature brittleness correlates with puncture failure on frozen product edges. Heat-seal initiation typically occurs at 95–110°C for overlap seals, and hot tack under ASTM F1921 is specified on vertical form-fill-seal lines running above 60 cycles/min. Direct food-contact compliance is established through FDA 21 CFR 177.1520 and EU 1935/2004, with specific migration testing under EU 10/2011; overall migration must not exceed 10 mg/dm² for the finished web.
In greenhouse cover production, the resin is dry-blended with 10–25 wt% LDPE and, where long-wave IR retention is required, 10–20 wt% EVA; DOWLEX 2267A contributes tear resistance and low-temperature flexibility that LDPE-rich blends lose under repeated wind loading. Films are blown at 150–200 µm gauge with a die gap of 1.8–2.2 mm and a BUR of 2.2:1–3.0:1. HALS loading of 0.3–0.6 wt% and a benzophenone or benzotriazole UV absorber at 0.1–0.3 wt% are standard, but anti-haze and anti-drip ester additives at 0.3–0.8 wt% can migrate and reduce surface tension below 35 mN/m, altering condensed water droplet contact angle. Tensile properties are tested under ISO 527-3 at 500 mm/min; transverse elongation is commonly specified above 700%, and tear resistance under ASTM D1922 is typically above 150 g for 180 µm film. Sulfur vapor from agricultural pesticides attacks polyethylene through chain oxidation; therefore, film exposed to sulfur fumigation requires higher HALS concentration, and lower-density resin is not a substitute for stabiliser chemistry. Published long-term UV lifetime data for this specific DOWLEX 2267A greenhouse configuration is limited; weather resistance is confirmed by ASTM G154 cycle testing and tensile retention before deployment rather than by supplier-supplied lifetime values.
A coextruded PE/PE laminate sealant web using DOWLEX 2267A as the sealant skin is produced for stand-up pouches and flow-wrap packaging where recyclability targets require replacement of PET or aluminium foil. A typical layer ratio places 10–25% of the total web as the sealant layer, with the remainder being an MDO-PE or BOPE print web and an LDPE-based core. Seal initiation begins at 85–105°C, and plateau seal strength under ASTM F88 on a 100 µm film is usually between 20 N/15 mm and 35 N/15 mm, depending on jaw profile and dwell. Octene-comonomer LLDPE has a narrow melting distribution relative to LDPE, so the seal layer tolerates a 10–15°C shift in seal-bar temperature without burn-through on lines running above 80 m/min. Hot tack under ASTM F1921 is specified because top-loading form-fill-seal machines require 1.5–2.5 N/15 mm within 0.2 s of bar release at 105°C. The sealant layer is formulated with 1000–3000 ppm silica antiblock and 300–800 ppm erucamide slip; excessive slip migrates into the seal interface and can reduce hermetic seal strength below 15 N/15 mm. Adhesive or extrusion lamination to the print web requires corona pre-treatment to 38–42 mN/m, and solventless adhesive bond strength under ASTM F904 must remain above 2 N/15 mm after 24 h at 50°C.
Extrusion of drum liners at blow-up ratios below 2.8:1 shifts orientation toward higher machine-direction tear, which is specified for 75–125 µm liners inside fibre and steel drums. The die gap is normally 1.4–1.8 mm, and melt temperature is held between 205°C and 230°C; on a 90 mm single-screw line with an L/D of 30:1, backpressure is frequently observed in the range of 220–340 bar depending on screen pack condition. Chemical compatibility is measured under ASTM D543 using representative product simulants; octene-comonomer LLDPE is generally assigned for dilute mineral acids and alkalis, but aromatic solvents and strong oxidisers require barrier coextrusion with polyamide or EVOH, where DOWLEX 2267A serves as the sealing and toughness layer, not as the barrier. Environmental stress crack resistance under ASTM D1693 Condition B is critical for liquid packaging; users commonly require no failure at 1000 h in 10% Igepal CO-630 at 50°C, though published values for this specific liner structure are limited. Drop testing per ASTM D5276 from 1.2 m at -20°C is specified because seams can fail in cold drop before film body puncture. A typical three-layer structure places HDPE skins at 10–20% each and a DOWLEX 2267A core at 60–80%, preserving chemical resistance while retaining side-seal strength above 25 N/15 mm under ASTM F88.
| Film structure | Typical gauge | Blow-up ratio | Die melt temperature | Additive loading |
|---|---|---|---|---|
| Heavy-duty sack | 120–180 µm | 2.2:1–3.0:1 | 210–240°C | 2000–5000 ppm silica, 300–1000 ppm erucamide |
| Frozen food web | 50–80 µm | 2.0:1–2.8:1 | 205–235°C | 1500–4000 ppm silica, 400–1000 ppm erucamide |
| Drum liner | 75–125 µm | 2.0:1–2.8:1 | 205–230°C | 1000–3000 ppm silica, 300–800 ppm slip |
Perforation of collation shrink film on high-speed lines raises a different set of requirements than heavy-gauge sacks. DOWLEX 2267A is let down at 50–70 wt% with LDPE and a small addition of 5–10 wt% ethylene-vinyl acetate to achieve a 20–35 µm web that will shrink under hot air at 120–140°C without melt-through at the perforation line. Blown film towers are run with a die gap of 1.0–1.4 mm and a BUR of 3.0:1–4.0:1 to increase transverse shrink force; machine-direction shrink tension is controlled by frost-line height and haul-off speed. Perforation geometry is rotary pin or blade type, with holes from 0.8 mm to 2.0 mm diameter, and the film is tested for Elmendorf tear under ASTM D1922 after perforation because notched tears can propagate at below 20 g if the web is overwound. Sealability on shrink bundling machines requires a lap seal with jaw temperature of 110–130°C; seal strength under ASTM F88 is less critical than hot tack under ASTM F1921 because packs are transferred under tension. Blocking is controlled with 2500–5000 ppm silica antiblock and 500–1200 ppm erucamide slip, but excessive slip reduces ink adhesion after corona treatment, so the surface is treated to 38–42 mN/m offline. Published data for specific perforated shrink performance with DOWLEX 2267A is limited.
Competitive Dow DOWLEX™ 2267A Linear Low Density Polyethylene, Blown Film Grade prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Dow DOWLEX™ 2267A Linear Low Density Polyethylene, Blown Film Grade is an ethylene–1-octene copolymer produced via solution polymerization and supplied as pellets for blown film extrusion. Published typical values for the grade include a density of 0.917 g/cm³ measured by ISO 1183-1:2019 or ASTM D792-20 and a melt mass-flow rate of 1.0 g/10 min at 190°C/2.16 kg measured by ISO 1133-1:2022 or ASTM D1238-20. The density places the material in the lower end of the LLDPE film density range, where the amorphous fraction contributes to impact toughness, while the melt flow rate is sufficiently high to avoid the extreme melt pressures associated with fractional-melt film grades. Because the product is linear and lacks the long-chain branching of high-pressure LDPE, its melt rheology and bubble stability must be managed differently on the blown film line. The 1-octene comonomer introduces hexyl branches, distinguishing the product from butene-based LLDPE grades that contain ethyl branches. That branch-length difference is not cosmetic; it alters the distribution of short-chain branching, crystallization behaviour during quench, and the resulting tie-molecule population in solidified film.
The product is specified in blown film structures where downgauging and high tear resistance are primary technical requirements. Typical end-use formats include heavy-duty shipping sacks, industrial liners, frozen food packaging, and lamination film for liquid and powder packaging. Qualification for these formats commonly uses film dart impact by ASTM D1709-22 or ISO 7765-2, Elmendorf tear by ASTM D1922-23 or ISO 6383-2, tensile properties by ASTM D882-22 or ISO 527-3:2018, and optical haze by ASTM D1003-21 or ISO 14782. These measured values are not intrinsic material constants; they vary with die gap, blow-up ratio, frost line height, cooling air velocity, and takeoff speed. A converter substituting this grade for LDPE should not assume that the same barrel temperatures and die gap will produce comparable film optics or bubble geometry.
The solution polymerization route used for DOWLEX™ 2267A typically yields a more uniform intermolecular comonomer distribution than some gas-phase butene LLDPE technologies. This uniformity is visible in thermal fractionation and in melting endotherm shape, and it influences seal initiation and hot tack. In a film structure with a sealant layer, the seal initiation temperature of DOWLEX™ 2267A must be measured on the specific coextruded or monolayer film, because seal strength depends on film thickness, substrate stiffness, and additive migration from adjacent layers. Seal tests are conducted under ASTM F88/F88M-23 with defined dwell time and seal pressure; hot tack can be assessed on laboratory hot-tack instruments and reported with cooling time and sealing temperature.
The relevant structural variable is short-chain branch length. Butene-based LLDPE grades carry ethyl branches, whereas DOWLEX™ 2267A carries hexyl branches from 1-octene. In the solid state, longer short-chain branches are more effective at modifying the crystalline and amorphous interface and increasing the number of interlamellar tie molecules during film quench. This mechanism is widely referenced in polymer science literature as the reason octene LLDPE films frequently show higher dart impact and tear strength than butene LLDPE films of the same density and melt flow rate. The effect is not linear with density; at 0.917 g/cm³, the crystalline fraction is relatively low, and the amorphous tie-chain network becomes a larger contributor to toughness. On blown film lines operating at a blow-up ratio above 2.5:1, biaxial orientation is more pronounced, and the octene-based branch structure can reduce the directional tear imbalance observed in some gas-phase butene resins.
Differences also appear in melt rheology. DOWLEX™ 2267A is produced with a broader molecular weight distribution than most metallocene-catalysed octene LLDPE grades, which improves processability on conventional extruders but does not necessarily produce the same optical clarity as a high-clarity metallocene film resin. The choice between DOWLEX™ 2267A and a metallocene LLDPE usually involves a trade-off between extrusion amperage, melt pressure, and film haze. If a converter requires haze below 5% in 25 µm film, a metallocene grade may be selected, while DOWLEX™ 2267A is specified where balanced toughness and extruder compatibility are more important. Published comparative data for all three resin families in the same film line configuration is limited, so the comparison should be based on the converter’s own blown film trial.
Capillary rheometry by ISO 11443:2021 provides shear viscosity curves for the melt. Linear PE typically exhibits a higher power-law index than branched LDPE in the 100–1000 s⁻¹ shear-rate range, meaning its apparent viscosity decreases less steeply with increasing shear rate. The practical consequence is that increasing screw speed on DOWLEX™ 2267A raises melt pressure more steeply than on high-pressure LDPE. The resin therefore demands attention to screw speed, barrel pressure, and drive load when a converter moves from LDPE to LLDPE on a fixed extruder.
On a single-screw blown film line with screw diameter 45 mm and L/D 30:1, typical barrel settings from feed to adapter are 170°C, 190°C, 210°C, and 220°C, with adapter and die held at 220°C to 230°C. Melt temperature at the extruder outlet is maintained between 190°C and 230°C. Below 190°C, solids-bed breakup and high screw torque may appear, especially when the screw has a shallow feed section or when high output is attempted. Above 240°C, the film line is more likely to accumulate oxidised gel at the die lip, and long residence time increases the probability of black specks and odour. The annular die gap is generally set between 1.0 mm and 2.5 mm; a narrower gap raises shear rate and may reduce haze but increases melt pressure, while a wider gap reduces pressure and permits thicker film at a given mandrel speed. Frost line height is set at 2 to 4 die diameters. Because linear resins have lower melt tension than LDPE, bubble stability requires a consistent external air supply and collapse-frame alignment. Sudden changes in cooling air or nip speed can induce bubble flutter or draw resonance, and the resulting thickness variation may violate the ±10% gauge tolerance used in many industrial liner specifications.
Thermal degradation of polyethylene in the melt is initiated primarily by oxygen rather than by simple thermal cleavage below 300°C. Radical chain scission and branching occur simultaneously; oxidation increases carbonyl absorbance, measurable by FTIR according to ASTM D5576-19. In a blown film die, stagnation zones at the mandrel or heater bands can create local hot spots above the barrel setpoint. Melt temperature at the die should therefore be measured with an immersion thermocouple, not inferred from controller settings. A rise of 5–10°C above the target can indicate shear heating, which becomes more important with high-output screws above 120 rpm. Gel specks in film can be counted by film inspection methods such as ASTM D3596-20; an elevated gel count after a run at high melt temperature indicates oxidative degradation or stagnant resin in the die.
Blending DOWLEX™ 2267A with high-pressure LDPE at 10–30 wt% LDPE is used to increase melt strength and widen the stable operating window on lines originally designed for LDPE. At 10 wt% LDPE addition, melt fracture onset at high output is generally suppressed, and higher blow-up ratios can be sustained without bubble collapse. The penalty is an increase in haze and a reduction in secant modulus as the long-chain branched LDPE component introduces a broader relaxation spectrum and lower crystallinity. At 30 wt% LDPE, the film begins to approach the shrinkage and optical behaviour of LDPE-rich blends, which can be useful for collation shrink and overwrap but may negate the downgauging advantage of the LLDPE component.
Blends with metallocene LLDPE at 20–40 wt% are more complex. The two components may have different melting and crystallization kinetics, and the sealing window of the blend is not simply the weighted average of the individual resins. Heat-seal initiation temperature and hot tack should be measured on the finished film using laboratory sealers and reported with seal pressure, dwell time, and specimen width; the broader melting distribution of DOWLEX™ 2267A can shift the seal initiation temperature upward relative to the metallocene component alone. If the blend is used in a form-fill-seal line, hot tack becomes a critical performance parameter because the seal must survive product loading before cooling. The converter should measure hot tack across the sealing temperature range and compare the failure mode with the production line dwell time and jaw pressure.
In 25 µm film, optical and mechanical performance is evaluated as a system property, not a resin property. Haze is measured by ASTM D1003-21 or ISO 14782, gloss at 45° by ASTM D2457-21, and secant modulus by ASTM D882-22. Dart impact is measured by ASTM D1709-22 using the staircase method. These test scores are affected by gauge uniformity, die-lip residue, and frost line oscillation. A converter evaluating the product for frozen food film typically records haze, gloss, dart impact, and low-temperature puncture; the latter is relevant because LLDPE film retains impact resistance at freezer temperatures better than some LDPE-rich structures.
No published data for every film configuration is available. When specific values are absent, the converter should generate a quality-control baseline using the same extruder, die, and takeoff speed as production. The product is often compared with higher-density LLDPE film grades, which have higher modulus but lower Elmendorf tear. These differences are captured in the test method matrix below.
| Parameter | Standard designation | Reported configuration |
|---|---|---|
| Melt mass-flow rate | ISO 1133-1:2022 / ASTM D1238-20 | 190°C/2.16 kg |
| Density | ISO 1183-1:2019 / ASTM D792-20 | 23°C, immersion |
| Film dart impact | ASTM D1709-22 / ISO 7765-2 | F50, 25 µm film |
| Elmendorf tear | ASTM D1922-23 / ISO 6383-2 | 25 µm film, MD/TD |
| Secant modulus | ASTM D882-22 / ISO 527-3:2018 | 25 µm film, MD/TD |
| Haze | ASTM D1003-21 / ISO 14782 | 25 µm film |
| Gloss | ASTM D2457-21 | 45°, 25 µm film |
Compared with fractional-melt LLDPE extrusion grades, the 1.0 g/10 min melt flow rate of DOWLEX™ 2267A reduces shear stress at the die lip at the same throughput, which lowers the tendency for melt fracture. The effect is more visible on narrow die gaps and at high output. However, the lower viscosity relative to fractional-melt resin also reduces bubble stability at very high blow-up ratios, because the molten film has less resistance to stretching in the machine direction. Processors therefore balance die gap, melt temperature, and blow-up ratio rather than relying on a single setting. On a 40 mm extruder, a die gap of 1.4 mm and a blow-up ratio of 2.5:1 are practical starting points; the frost line is adjusted to maintain bubble symmetry and to control roll blocking in films produced without added antiblock.
Die-lip deposit formation commonly results from low molecular weight species, additives, or degraded gel. The cleaning interval should be established during a production trial and should account for the particular die gap and melt temperature. If the die-lip deposit increases rapidly, the converter should measure melt temperature at the die exit and inspect the screw for wear or stagnant zones. Screw wear in high-throughput lines changes melt homogeneity and can raise the local melt temperature even when barrel controllers remain unchanged.
Operational boundaries should be documented. The resin should be protected from condensation during silo or gaylord storage; although polyethylene is not hygroscopic, surface moisture introduced in high-humidity environments can cause bubble pinholes. If surface moisture is suspected, pellets can be dried at 60°C for 2 h in a desiccant or hot-air dryer, but prolonged drying is not required. The melt should not be held above 240°C for more than 20 min during interruptions. Extruder shutdown and purge procedures should use a lower-density polyethylene purge material to displace the linear resin from the screw, adapter, and die; this reduces the risk of gel accumulation in stagnant zones. The product is not compatible with prolonged exposure to strong oxidising agents; storage should avoid contact with open flame and ultraviolet-activated oxidising vapours. These limitations are standard for polyethylene film extrusion and are relevant when the resin is used in high-output operations with minimal purge time.
For food-contact applications, the resin may be used by converters only after verification that the finished article complies with FDA 21 CFR 177.1520 for olefin polymers and EU Regulation 10/2011 as amended, including overall migration and specific migration limits for the intended food simulant and contact duration. The supplier’s product-specific certification should be consulted because additive lot variations and downstream printing adhesives affect final compliance. REACH registration obligations apply to the product placed on the European market, and the converter is responsible for verifying that the imported film article does not exceed the restricted substance limits under REACH Annex XVII.