| HS Code | 269881 |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Grade | Blown Film |
| Density | 0.920 g/cm3 |
| Melt Index 190 C 2 16 Kg | 0.70 g/10 min |
| Melting Point Dsc | 122 °C |
| Vicat Softening Point | 100 °C |
| Tensile Strength At Yield Md | 11 MPa |
| Tensile Strength At Yield Td | 11 MPa |
| Tensile Strength At Break Md | 32 MPa |
| Tensile Strength At Break Td | 30 MPa |
| Elongation At Break Md | 700% |
| Elongation At Break Td | 800% |
| Elmendorf Tear Strength Md | 250 g |
| Elmendorf Tear Strength Td | 450 g |
| Dart Drop Impact | 200 g |
| Haze | 8% |
| Gloss 45 | 60 |
| Coefficient Of Friction | 0.20 |
| Blocking | 35 g |
As an accredited Dow DOWLEX™ 2101 Linear Low Density Polyethylene, Blown Film Grade factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Dow DOWLEX™ 2101 is packaged in 25 kg polyethylene-lined paper bags, supplied on stretch-wrapped pallets for industrial use. |
| Container Loading (20′ FCL) | 20′ FCL loads about 20 MT of Dow DOWLEX™ 2101 LLDPE blown film grade in 25 kg bags (800 bags). |
| Shipping | DOWLEX™ 2101 LLDPE is typically shipped in 25 kg moisture-resistant bags, palletized, or in 1,000 kg bulk containers. Bulk trucks or railcars may be used. Transport clean, dry, away from heat, sunlight, moisture, and incompatible materials. Not classified as hazardous for normal transport. |
| Storage | Store DOWLEX™ 2101 in a cool, dry, well-ventilated, covered area away from direct sunlight, moisture, heat, sparks, and oxidizers. Keep original bags/containers closed and off the floor on pallets to prevent contamination and moisture pickup. Avoid excessive stacking. Use first-in, first-out inventory. Maintain normal ambient temperatures; avoid prolonged storage near strong odors or ignition sources. |
| Shelf Life | Shelf life: 24 months when stored in original unopened packaging in a cool, dry, well-ventilated area away from direct sunlight. |
Film extruded from DOWLEX™ 2101, specified at melt index 1.0 g/10 min per ASTM D1238-20 and density 0.920 g/cm³ per ASTM D792-20, is converted into frozen-food pouches at distribution temperatures between -25°C and -18°C. The typical formulation is 80-100 wt% DOWLEX™ 2101 with 0-20 wt% LDPE and 2-4 wt% slip/antiblock masterbatch. A single-screw extruder with barrier screw at L/D 30:1, die gap 1.8-2.2 mm, die diameter 200-300 mm, melt temperature 190-225°C, BUR 2.0-2.5, frost-line height 18-30 cm above the air ring, and gauge 50-70 µm is used. The film is corona-treated to 38-42 mN/m, and slip/antiblock masterbatch maintains coefficient of friction below 0.30 per ASTM D1894-14. Downstream conversion includes flexographic or rotogravure printing and form-fill-seal packaging at seal jaw temperatures of 120-150°C and seal dwell times of 0.5-1.2 s. Food-contact compliance is anchored to FDA 21 CFR 177.1520(c) 3.2a, EU Regulation 10/2011 with overall migration limit 10 mg/dm² tested by EN 1186-1:2002, and GMP under 21 CFR 174.5. Terminal products include printed pouches for frozen vegetables, seafood, and bakery items. Processing limitation: melt temperatures above 225°C increase gel formation in the octene-copolymer matrix and reduce heat-seal hot tack at the form-fill-seal stage; below 190°C, die-head pressure rises and output per die circumference drops below 1.5 kg/h/mm unless a pressure-compensated screw design is used.
In heavy-duty industrial packaging, DOWLEX™ 2101 is formulated at 70-90 wt% with 10-30 wt% recycled LLDPE or HDPE and 2-4 wt% processing aid masterbatch, then extruded on a three-layer coextrusion blown film line with screw L/D 30:1, die gap 2.0-2.8 mm, BUR 2.0-2.8, melt temperature 200-230°C, and gauge 100-150 µm. The downstream process includes in-line gusseting, surface treatment to 38-42 mN/m, and conversion into shipping sacks by heat sealing or sewing. Compliance for the product class is specified by ASTM D1709-16a Method A for dart impact, ASTM D1922-15 for Elmendorf tear, ASTM D882-18 for tensile strength, ISO 21898 for FIBC-grade liners, and UN 13H2 certification under ADR/RID for hazardous goods. A process conflict exists between impact and tear orientation: increasing BUR from 2.0 to 2.8 improves TD Elmendorf tear but may reduce MD tear below 30 N/mm if frost-line height exceeds 3 times the die diameter. Terminal products include FIBC inner liners, heavy-duty gusseted sacks, and hazardous waste disposal bags. The inclusion of post-industrial reclaim above 30 wt% introduces gel-count variability that destabilizes bubble geometry and lowers dart impact below 200 g; published data for DOWLEX™ 2101 with this specific reclaim level is limited, so blender-side trials are required.
For agricultural silage bale wrap and silage cover film, DOWLEX™ 2101 is compounded at 70-85 wt% with 15-30 wt% LDPE or EVA, plus a UV-stabilizer masterbatch at 5-8 wt% containing hindered amine light stabilizers, and extruded on a three-layer blown film line with die gap 2.0-2.5 mm, BUR 2.0-3.0, melt temperature 190-215°C, and gauge 100-200 µm. The downstream process uses a round-bale wrapper with a pre-stretch unit applying 60-80% elongation to the film before wrap, so the film must have tensile elongation at break of at least 350% per ASTM D882-18 and dart impact adequate for puncture from crop stems. In the field, compliance is specified under EN 14932:2018 for stretch thermoplastic films for wrapping bales and EN 13206:2017 for covering films in agriculture; UV durability is screened by exposure in ISO 4892-2 cycle 1 for 2000 h with tensile retention above 70% of original MD strength. Terminal products are round-bale silage wrap, fermentation covers, and temporary greenhouse side curtains. Operational boundary: processing above 220°C may reduce the efficiency of the hindered amine light stabilizer package; published data for DOWLEX™ 2101 in this specific UV-stabilized configuration is limited, and converter trials should verify field lifetime.
Blown film produced from DOWLEX™ 2101 at 25-50 µm is used as the heat-seal layer in adhesive-laminated flexible packaging. The film is formulated at 85-100 wt% DOWLEX™ 2101 with 0-15 wt% LDPE to increase melt strength, and 2-4 wt% antiblock masterbatch to prevent roll blocking after corona treatment to 38-42 mN/m. Extrusion parameters are die gap 1.5-2.0 mm, BUR 2.0-2.5, melt temperature 195-220°C, and gauge variation below ±10%. The downstream process is adhesive lamination to PET 12 µm or BOPP 18 µm using solventless polyurethane adhesive at a coat weight of 1.5-2.5 g/m²; the LLDPE sealant surface is then tested for heat-seal strength by ASTM F88/F88M-21 at seal temperatures of 85-120°C, pressure of 0.30-0.45 MPa, and dwell 0.5 s. Food-contact compliance for the sealant web is based on FDA 21 CFR 177.1520 and EU Regulation 10/2011; the adhesive system must separately comply with 21 CFR 175.105 where indirect food contact applies. Terminal product types include stand-up pouches for dry foods, frozen fruit, and pet treats. Operational limitation: a coefficient of friction above 0.35 per ASTM D1894-14 induces registration drift on pouch-making machines; slip migration in the LLDPE matrix may require 48-72 h at 25°C to reach stable coefficients after conversion.
Collation shrink film made with DOWLEX™ 2101 uses 60-80 wt% DOWLEX™ 2101 blended with 20-40 wt% LDPE and 2-3 wt% slip/antiblock, is blown at die gap 1.8-2.2 mm, BUR 2.0-2.5, melt temperature 180-210°C, and gauge 30-50 µm, then is passed through a shrink tunnel at 140-160°C; free shrink per ASTM D2732-14 Method A is typically 12-18% MD and 15-20% TD, depending on frost line. Compliance for beverage multipack collation sleeves is covered by EU Packaging Directive 94/62/EC and EN 13430 for packaging material recovery; terminal products include printed shrink sleeves for bottle multipacks and can collation wraps. Published data for DOWLEX™ 2101 in high-stalk shrink orientation is limited; production trials determine final shrink percentages and tunnel speed.
| Application | DOWLEX 2101 loading | Co-resin level | Melt temperature | Die gap | BUR | Typical gauge |
|---|---|---|---|---|---|---|
| Frozen-food pouches | 80-100 wt% | LDPE 0-20 wt% | 190-225°C | 1.8-2.2 mm | 2.0-2.5 | 50-70 µm |
| Heavy-duty shipping sacks | 70-90 wt% | Recycled LLDPE/HDPE 10-30 wt% | 200-230°C | 2.0-2.8 mm | 2.0-2.8 | 100-150 µm |
| Agricultural silage wrap | 70-85 wt% | LDPE/EVA 15-30 wt% | 190-215°C | 2.0-2.5 mm | 2.0-3.0 | 100-200 µm |
| Lamination sealant web | 85-100 wt% | LDPE 0-15 wt% | 195-220°C | 1.5-2.0 mm | 2.0-2.5 | 25-50 µm |
| Collation shrink film | 60-80 wt% | LDPE 20-40 wt% | 180-210°C | 1.8-2.2 mm | 2.0-2.5 | 30-50 µm |
| Wet-cut ice bags | 90-100 wt% | LDPE 0-10 wt% | 185-210°C | 1.5-2.0 mm | 2.5-3.5 | 37-50 µm |
| Application | Standard or regulation | Method / clause | Typical requirement |
|---|---|---|---|
| Frozen-food pouches | FDA 21 CFR 177.1520 | c 3.2a | Overall migration 10 mg/dm² per EU 10/2011 |
| Heavy-duty shipping sacks | ASTM D1709-16a | Method A | Dart impact acceptance often 250 g at 125 µm |
| Agricultural silage wrap | EN 14932:2018 | Bale wrap performance | Tensile elongation ≥350% per ASTM D882-18 |
| Lamination sealant web | FDA 21 CFR 177.1520 | Sealant layer | Heat-seal strength by ASTM F88/F88M-21 |
| Collation shrink film | EN 13430 | Packaging material recovery | Free shrink 12-20% per ASTM D2732-14 |
| Wet-cut ice bags | FDA 21 CFR 177.1520 | Polyolefin food-contact | Haze ≤8% per ASTM D1003-21 |
Ice bag conversion of DOWLEX™ 2101 uses a formulation of 90-100 wt% DOWLEX™ 2101 and 0-10 wt% LDPE, with antiblock masterbatch at 1-2 wt% and slip masterbatch at 0.5-1.5 wt%; antiblock addition above 2 wt% reduces 45° gloss below 50 per ASTM D2457-21 and raises haze above 8% per ASTM D1003-21. The blown film process uses a die gap 1.5-2.0 mm, BUR 2.5-3.5, melt temperature 185-210°C, and gauge 37-50 µm; the high BUR increases transverse-direction tear resistance for filled wet ice weights up to 10 kg. Downstream conversion includes bag forming, perforation, and heat sealing at 110-130°C. Compliance for wet ice contact is based on FDA 21 CFR 177.1520 for polyolefins in food-contact applications and EU Regulation 10/2011 where applicable. Terminal products include drawstring ice bags, block ice bags, and freezer-grade consumer bags. Operational boundary: at BUR 3.5, bubble stability on production lines without internal bubble cooling is reduced unless melt temperature is kept at the lower end of the range and output is limited to 1.5 kg/h per mm die circumference to avoid film wander.
Competitive Dow DOWLEX™ 2101 Linear Low Density Polyethylene, Blown Film Grade prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Among ethylene-α-olefin copolymers used in monolayer and coextruded blown film, DOWLEX™ 2101 Linear Low Density Polyethylene is a solution-polymerized ethylene-octene product supplied as pellets with a nominal melt index of 1.0 g/10 min per ASTM D1238 or ISO 1133-1 at 190 °C/2.16 kg and a nominal density of 0.919 g/cm³ per ASTM D1505 or ISO 1183-1. The grade is designated for blown film because its moderate molecular weight and octene short-chain branching distribution provide a balance among tear resistance, dart impact strength, and drawdown on air-cooled film lines. Unlike high-pressure low-density polyethylene, which contains long-chain branching, DOWLEX 2101 has a predominantly linear backbone; this reduces strain hardening and makes bubble stability dependent on frost-line control, air-ring geometry, and die-gap settings rather than on the extensional-strain-hardening response typical of tubular or autoclave LDPE.
Typical application areas include industrial liners, heavy-duty sacks, frozen-food packaging, form-fill-seal webs, and surface layers in coextruded structures where toughness and seal performance are required. The product is often selected over butene-based LLDPE because the octene comonomer produces a higher concentration of stress-transmitting tie molecules between crystalline lamellae. This structural difference raises Elmendorf tear and dart impact values at equal density and melt index when measured by ASTM D1922 and ASTM D1709. The resin is naturally translucent; haze and gloss must be verified by the converter because film optics depend on die-gap, blow-up ratio, frost-line height, and cooling-air temperature. For food-contact packaging, the base olefin polymer falls under the general clearance framework of 21 CFR 177.1520(c), but finished-package migration testing under EU Regulation No 10/2011 and applicable national legislation remains the responsibility of the converter or brand owner.
On a standard 75 mm to 90 mm grooved-feed single-screw extruder with a 24:1 to 30:1 L/D barrier screw and a spiral-mandrel die, DOWLEX 2101 is normally processed with a feed-throat temperature below 50 °C, a barrel profile from 180 °C to 220 °C, adapter zones at 220 °C, and die zones at 220–250 °C. Die-head pressures are typically higher than those of an equivalent-melt-index LDPE by 15–30% because the linear polymer does not shear-thin to the same extent. Motor amperage and melt-pressure variation should be monitored against the extruder drive limit when increasing screw speed. A die-exit melt temperature of 220–235 °C is a practical operating window; below 210 °C the risk of shark-skin melt fracture on untreated die lips increases, while above 250 °C oxidation can generate gel particles, reduce tear strength, and increase odour potential.
Die gap is commonly set at 1.6–2.0 mm for film gauges from 25 µm to 125 µm. A blow-up ratio of 2.0:1 to 3.0:1 and a frost-line height of 5–8 die diameters are typical for balanced machine-direction and transverse-direction properties. Higher frost lines improve transverse-direction tensile strength but weaken bubble stability. Dual-lip air rings and internal bubble cooling are recommended when output exceeds approximately 1.5 kg/h per cm of die circumference. At higher specific outputs, bubble oscillation and gauge variation can develop unless the die land length and air-ring volume are sufficient to stabilise the tubular film. If gauge variation exceeds ±5% on a film scanner, screw speed should be reduced or frost-line height increased; raising melt temperature alone is not an effective remedy because it further reduces the already limited melt strength of the linear resin.
Because the linear microstructure lacks the strain-hardening plateau of autoclave or tubular LDPE, the frost line is particularly sensitive to radial air-velocity distribution. Unstable bubbles often appear as helical or vertical diameter oscillation when the cooling-air rate is too high at a low frost-line position. On production lines with internal bubble cooling, the internal air temperature should be maintained at 20–35 °C and the exhaust rate adjusted to avoid ballooning. In closed-loop gauge control, haul-off speed and blow-up ratio should be integrated with the die-bolt heating zones, particularly when running films below 35 µm. Purging after shutdown is conventionally performed with a fractional-melt HDPE or a commercial purge compound, followed by the resin itself, because the linear polymer can remain in the spiral-mandrel channels if the die is cooled too rapidly.
Resin drying is not normally required unless surface condensation has occurred during storage in high-humidity environments. If moisture is visible, pre-drying for 2–4 h at 70–80 °C in a desiccant-bed hopper dryer is sufficient. Extended drying at higher temperatures should be avoided because pellet surface oxidation can occur even before the polymer enters the extruder. Dust and fines should be removed at the hopper vent to reduce gels.
Film property comparisons are meaningful only when processing conditions and test thickness are controlled. The following matrix summarises the relative response of DOWLEX 2101 against high-pressure LDPE and butene LLDPE at comparable melt index and film gauge. The comparisons are based on industrial film-testing practice; absolute values vary with blow-up ratio, frost-line height, die gap, and laboratory conditioning.
| Property | Test method | DOWLEX 2101 versus high-pressure LDPE at comparable MI | DOWLEX 2101 versus butene LLDPE at comparable MI |
|---|---|---|---|
| Dart impact resistance | ASTM D1709 | Higher | Higher |
| Elmendorf tear strength | ASTM D1922 | Higher | Higher |
| Tensile strength at break | ASTM D882 | Higher | Comparable to slightly higher |
| Puncture resistance | ASTM D5748 | Higher | Higher |
| Haze | ASTM D1003 | Higher | Comparable |
| Gloss at 45° | ASTM D2457 | Lower | Comparable |
| Melt strength and bubble stability | Rheotens or line observation | Lower | Comparable to slightly lower |
Film converters commonly measure seal initiation temperature with a gradient heat-seal apparatus in which dwell time, sealing pressure, and temperature are controlled. For DOWLEX 2101, the seal initiation temperature is generally higher than that of a high-pressure LDPE and lower than that of a high-density polyethylene. Because the grade is an octene copolymer with a density of 0.919 g/cm³, the sealant layer remains tacky over a wider temperature range than a high-density sealant, which improves seal-through-contamination performance in form-fill-seal packaging. Hot-tack strength is commonly assessed by ASTM F1921 or equivalent plant-specific methods, and the optimal hot-tack plateau is obtained only when the heat-seal jaw temperature is kept below the point at which the sealant thins excessively and begins to squeeze out of the seal area.
Property values for a specific film configuration should not be inferred from raw resin data alone. Published data for film properties at non-standard blow-up ratios or at very high output rates are limited; converters should establish their own correlations between frost-line height, bubble stability, and tear balance using statistically valid sampling plans. The resin specification checklist below provides the incoming quality-control and regulatory verification framework commonly used by film plants.
| Control item | Reference or standard designation | Verification expectation |
|---|---|---|
| Melt mass-flow rate | ASTM D1238 / ISO 1133-1 | 1.0 g/10 min nominal at 190 °C/2.16 kg; lot-specific limits per purchase specification |
| Density | ASTM D1505 / ISO 1183-1 | 0.919 g/cm³ nominal |
| Peak melting temperature | ASTM D3418 | Typical polyethylene melting range; not used as a lot-release criterion |
| Food-contact olefin polymer clearance | 21 CFR 177.1520(c) | End-user migration validation required for finished package |
| European food-contact plastics | EU Regulation No 10/2011 | Specific migration limits for ethylene and octene-1 must be assessed under intended food simulants |
| Heavy metals restrictions | EU Directive 2011/65/EU | No intentionally added restricted substances; verify via supplier declaration |
The difference in tear balance between machine direction and transverse direction is controlled by the blow-up ratio and frost-line height rather than by the resin alone. At a low blow-up ratio of 1.5:1, machine-direction orientation increases and transverse-direction tear strength may fall below converter targets, while at 3.0:1 the opposite occurs. DOWLEX 2101 does not contain an antiblock or slip additive as a default; masterbatch addition rates for antiblock, slip, or processing aid must be determined on the production line because the linear polymer requires adequate surface treatment and melt-fracture suppression when running at high shear rates.
When DOWLEX 2101 replaces a high-pressure LDPE in a coextruded blown film layer, the extrusion engineering team must first evaluate layer ratio, die temperature, and air-ring settings. In a three-layer line with a polyamide or EVOH barrier core, the linear polyethylene sealant layer may require a higher die-head pressure and a slightly wider die gap than an LDPE sealant of the same melt index. If the die-gap is not widened, the linear layer can generate interfacial instability at high output because of the viscosity mismatch with the barrier polymer. The practical remedy is to raise the die temperature by 5–10 °C or increase the sealant-layer die gap while maintaining the same total film gauge.
Compared with a high-pressure LDPE sealant, the octene-based LLDPE sealant layer improves dart impact and puncture resistance but reduces optical clarity. In coextruded frozen-food packaging, the lower water-vapour transmission rate of the linear polyethylene may be marginal because the primary barrier function is supplied by the core layer. The more significant operational difference is hot-tack behaviour at high packaging speeds: the DOWLEX 2101 sealant layer retains seal strength over a broader jaw-temperature interval, but it also produces a stiffer bubble and more visible die-lines if pigmented or if processing aid is insufficient. Processors should monitor seal-bar pressure and anvil temperature because the linear polymer requires slightly higher heat input than a branched LDPE to achieve the same seal strength at a given dwell time.
Differences between DOWLEX 2101 and other linear low-density polyethylene grades arise mainly from comonomer type and molecular-weight distribution. Butene-based LLDPE of similar density and melt index typically shows lower dart impact and lower Elmendorf tear because the shorter butene branch is less effective at forming tie-molecules in the amorphous phase. Hexene-based grades occupy an intermediate position, while octene-based DOWLEX 2101 provides higher toughness at the same density. Metallocene-catalysed LLDPE grades often show improved optical properties and lower extractables because of narrow molecular-weight and comonomer distributions, but they may also show lower bubble stability on conventional blown film equipment designed for broader-distribution Ziegler-Natta resins. DOWLEX 2101 is therefore specified when film toughness and broad processing latitude are more important than ultimate optical quality.
For extruder operators, the last point is practical: the resin should be run at a stable screw speed and not over-sheared. Long residence times at high die temperatures above 250 °C can crosslink or degrade the polymer and create gel strings in the film. The safest operating sequence is to start at a moderate screw speed, establish the frost-line height at 6–7 die diameters, then raise output while watching die-head pressure and bubble diameter. If bubble oscillation develops, the first adjustments should be air-ring volume and frost-line height, not melt temperature.