| HS Code | 629043 |
| Density | 0.920 g/cm³ |
| Melt Index 190 C 2 16 Kg | 1.0 g/10 min |
| Melt Flow Ratio I21 I2 | 30 |
| Tensile Strength At Yield | 10.3 MPa |
| Tensile Strength At Break | 24.1 MPa |
| Elongation At Break | 700% |
| Flexural Modulus 1 Secant | 241 MPa |
| Vicat Softening Point | 93°C |
| Brittleness Temperature | < -70°C |
| Environmental Stress Crack Resistance 10 Igepal | >1000 h |
| Hardness Shore D | 48 |
| Thermal Conductivity | 0.35 W/m·K |
As an accredited Dow DOWLEX™ 2071 Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Dow DOWLEX™ 2071 LLDPE is supplied in 25 kg polyethylene bags, palletized, or 1,000 kg bulk bags. |
| Container Loading (20′ FCL) | 20′ FCL: 20 MT Dow DOWLEX™ 2071 LLDPE in 25 kg bags, palletized, shrink-wrapped, and secured with straps. |
| Shipping | Dow DOWLEX™ 2071 Linear Low Density Polyethylene is shipped as non-hazardous solid resin pellets in sealed bags, boxes, or bulk containers. Transport by truck, rail, or sea in dry, clean conditions. Avoid moisture, excessive heat, direct sunlight, and contamination. No special hazardous-materials placards required. |
| Storage | Store DOWLEX™ 2071 linear low density polyethylene in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, sparks, flames, and strong oxidizing agents. Keep original bags or containers tightly closed to prevent moisture, dust, and contamination. Avoid excessive stacking and temperature extremes. Maintain clean, segregated storage, follow local regulations and the SDS, and use first-in, first-out stock rotation. |
| Shelf Life | Typically 24 months when stored in original unopened packaging in a cool, dry, well-ventilated area away from direct sunlight and heat. |
Five-layer cast stretch film allocation for DOWLEX 2071 is defined by draw ratio and edge hold rather than by melt index alone. The resin is metered into core or sub-skin layers at 40–70 wt% because octene-based short-chain branching in the DOWLEX resin delays strain hardening under web acceleration, and the density of 0.920 g/cm³ (ISO 1183-1) supplies enough crystallinity to resist edge tear. Melt index, measured as 2.3 g/10 min at 190 °C/2.16 kg (ISO 1133-1:2022), enables high throughput without excessive polymer backpressure on lines equipped with 75 mm and 90 mm 30:1 L/D extruders. Barrel profiles are set from 190 °C at the feed section to 245 °C at the metering section; die temperature is controlled at 245 °C, and the chill roll is maintained at 22–26 °C. Air knife pressure of 3.5–5.0 bar and vacuum box suction of -0.5 to -0.8 bar are used to pin the web to the primary chill roll at take-off speeds of 800–1,100 m/min. Sheets wound above 2,500 mm jumbo diameter use taper tension from 70% to 45% of set unwind value to prevent blocking.
Erucamide is not compounded into the DOWLEX 2071 pellet at the reactor; converters add a masterbatch in the outer cling layer or saturate the core only when a two-sided cling specification is required. At core addition levels above 500 ppm, migration from the core into the interface produces internal slip planes that lower transverse tear energy after film ageing. The effect is evaluated by Elmendorf tear (ASTM D1922) and tensile testing (ASTM D882); if tear values fall below 2.5 N/mm in the transverse direction after 8 weeks of warehouse storage at 23 °C, the core amide concentration is reduced or the release skin thickness is increased by 2–3 µm. Haze is measured at 23 µm thickness according to ASTM D1003; structures with silica-based anti-block at 1,000–2,000 ppm in the skin typically maintain haze below 2.0%. Puncture resistance is assessed by ASTM D5748; the energy at break on a 19 mm probe at 250 mm/min is evaluated on every production campaign because differences in quench rate alter the core-skin crystalline orientation.
| Position | Resin allocation | Nominal thickness (µm) | Additive loading (ppm) | Function |
|---|---|---|---|---|
| A | mLLDPE cling | 1.5–2.5 | 2,000–4,000 erucamide | peel cling |
| B | DOWLEX 2071 | 7.0–10.0 | 0–500 silica | draw resistance |
| C | DOWLEX 2071 | 2.0–4.0 | 1,000–2,000 silica | slip |
| D | mLLDPE release | 1.5–2.5 | 1,500–3,000 silica | unwind |
| Total film | — | 12–23 | — | pallet load retention |
During start-up, the first 50 kg of film after purging is held for optical inspection because transition material can contain gel-like specks from the previous metallocene grade. DOWLEX 2071 is supplied in stabilised pellet form; no predrying is required before processing, but condensation from cold silo storage into a warm extrusion hall can produce surface moisture. Silos are kept above 15 °C and purge air dew point below -20 °C to prevent feed slip and melt pressure oscillations exceeding ±10 bar on the core extruder. Post-industrial trim at up to 15 wt% is commonly reintroduced into the core layer without loss of visual quality if the fluff is densified and metered through a side feeder; higher reclaim loads raise gel count and puncture variability.
In refrigerated and frozen poultry packaging, a 16–25 µm film containing DOWLEX 2071 is subjected to bone-edge puncture at deep-chill and frozen storage temperatures. The resin’s octene-based comonomer increases amorphous-phase mobility at low temperature relative to a C4-LLDPE of equal density; dart impact retention after 48 h at -18 °C is tested under ASTM D1709 Method A. Direct side-by-side data for DOWLEX 2071 under identical blown or cast film conditions is limited; however, comparative plant trials with a butene LLDPE control repeatedly show that the octene-copolymer structure reduces the loss of impact energy at -18 °C when the film is not over-stretched during winding. The main process restriction is melt temperature: die temperatures above 260 °C create oxidative by-products, and sensory evaluation of sealed packs by DIN 10955 may reveal off-odour when the film was sealed at 135 °C for 1 s. In horizontal form-fill-seal operations running 60–90 packs/min, web flutter is controlled by using 23 µm film for bone-in cuts rather than 18 µm, adding mass without changing the seal profile because the DOWLEX 2071 layer is buried in the core.
| Standard/regulation | Test method | Condition | Acceptance criterion |
|---|---|---|---|
| FDA 21 CFR 177.1520 | Olefin polymer end-testing | Intended food simulants and temperatures | No exceedance of migration limits |
| EU 10/2011 | Overall migration | Frozen-food simulant condition | ≤ 60 mg/kg |
| DIN 10955 | Sensory panel | Sealed pack 135 °C, 1 s | No off-odour above panel threshold |
Seal initiation in coextrusions with a metallocene plastomer sealant is measured by ASTM F1921 and ASTM F88. Hot-tack strength above 2.0 N/25 mm is normally recorded only after seal bar temperature exceeds 105 °C; below that, peeling at the interface predominates over cohesive failure. DOWLEX 2071 functions as the stiffness-generating core layer, permitting a reduction in total film thickness from 25 µm to 20 µm while retaining the same bending stiffness at the back-fin seal. Food-contact compliance must be verified on the final structure under FDA 21 CFR 177.1520 and EU 10/2011; the pellet does not automatically confer compliance to coextruded films containing migrating slip agents, tie resins, or recycled edge trim. Overall migration testing according to EU 10/2011 is performed at the intended food simulant and time-temperature condition; for frozen poultry, simulant A or 95% ethanol at 20 °C for 10 days is not automatically representative and must be replaced by the frozen-food condition in the regulatory risk assessment.
Where palletised goods are secured by stretch hood equipment, the film is drawn over load corners at ratios that exceed 70:1 and must retain containment force during transport. DOWLEX 2071 is used in stretch hood film in blends with polar-free polyolefin plastomers; the LLDPE fraction contributes yield stress and puncture resistance, while the plastomer fraction distributes elongation and reduces stress whitening at the point of maximum draw. Holding force is measured at 100% elongation on a 500 mm strip according to ASTM D5459; industrial formulations containing 60–80 wt% DOWLEX 2071 typically show holding force in the 8–14 N/50 mm range, with the lower boundary observed when film temperature exceeds 40 °C immediately after the stretch-hood cycle. Creep retention is measured by holding the film at 50% elongation for 24 h at 23 °C; the residual force in DOWLEX 2071-rich films is generally 60–75% of the initial value, whereas plastomer-rich films may retain above 80% but start from a lower initial force. This trade-off sets the practical upper DOWLEX 2071 content at around 80 wt% for loads with sharp corners and high stack weights.
Process stability depends more on the air knife and vacuum box than on the polymer melt. At the die, the melt curtain must be pinned without edge neck-in exceeding 15% of die width; this is achieved with an air knife pressure of 3.5–5.0 bar and vacuum box negative pressure of at least -0.6 bar. The chill roll temperature is set lower than that of pallet stretch film, typically 18–22 °C, to preserve orientation and reduce blocking in the wound roll. When the line stops, film remaining on the primary chill roll for more than 2 min develops transverse gauge bands; the restart procedure discards the affected section. DOWLEX 2071 does not require predrying, but high ambient relative humidity above 60% can create surface condensation on cold pellets in the hopper, causing screw feed surges of ±8 rpm on gravimetric systems; hopper purging with dehumidified air at -20 °C dew point removes this disturbance.
Extrusion coating of paperboard for frozen seafood sleeves uses DOWLEX 2071 at coating weights from 12 g/m² to 25 g/m² on a tandem extrusion line with a 120 mm 30:1 L/D extruder and a slot die set at 300–320 °C. The melt index of 2.3 g/10 min is higher than conventional LDPE coating grades; melt pressure at the die is correspondingly 20–40 bar lower than that of a broad-molecular-weight LDPE at equal output, but the narrow molecular weight distribution can widen edge neck-in if the die-to-nip distance is excessive. At 100 m/min with a 150 mm die-to-nip distance, neck-in is typically 20–35 mm. Reducing the die gap to 0.5 mm and holding the air gap below 90 mm narrows neck-in by 5–10 mm; line speeds above 250 m/min require blending 10–20 wt% LDPE or another high-melt-strength polymer to suppress draw resonance.
Adhesion to paperboard is evaluated by 180° peel according to ASTM D903. With corona treatment at 2–3 kW and ozone application of 1.0–2.5 g/h per metre web width, peel values above 8 N/15 mm are commonly reached; below 4 N/15 mm, the paperboard surface is either under-treated or the melt temperature is too low to generate oxidised species. Frozen-storage performance is measured by conditioning the coated board at -20 °C for 48 h and bending the scored blank; flaking or delamination indicates inadequate adhesion. DOWLEX 2071 is not a high-barrier layer; in seafood sleeves the polymer layer acts primarily as a water-resistant exterior and split-resistant coating, so oxygen and moisture vapour transmission rates remain governed by the paperboard and any inner barrier layer. The final structure must be checked for total migration under EU 10/2011 and for chloroform-soluble extractives under 21 CFR 177.1520 if the board is intended for direct food contact.
When DOWLEX 2071 is blended at 30 wt% into a three-layer heavy-duty sack coextrusion, the output window is limited by bubble stability rather than extruder torque. A 70 mm 30:1 L/D barrier screw with a 200 mm die and a 2.2:1 blow-up ratio processes the blend at melt temperatures of 190–220 °C. Raising the die temperature above 230 °C thins the melt and induces bubble sag before the frost line. The frost line height is set between 600 mm and 850 mm on a 360° rotating die; below 600 mm, transverse direction toughness declines, while above 850 mm, gauge uniformity deteriorates and the bubble becomes sensitive to cooling air fluctuations. Extruder barrel temperatures fall from 180 °C at the feed section to 220 °C at the adapter, and die temperature is kept below 230 °C. Specific energy input is typically 0.18–0.24 kWh/kg, and melt pressure before the screen changer ranges from 280 bar to 360 bar depending on filter pack condition.
Sack films at 120 µm thickness with 30 wt% DOWLEX 2071 and 70 wt% bimodal HDPE are tested by ISO 527-3 for tensile properties, ISO 6383-2 for tear resistance, and ISO 7765-1 for dart drop. Addition of 1.5 wt% carbon black masterbatch for UV protection raises the frost line by 100–150 mm because carbon black particles nucleate crystallisation and alter bubble geometry. Weathering resistance is evaluated by tensile elongation retention after 2,000 h of ISO 4892-2 cycle A exposure; retention above 70% is typically required for export sack storage in open yards. The primary incompatibility in this application is with acid-functional metal-neutralised ionomer scrap; residual metal ions accelerate oxidative degradation at 250 °C, produce gels, and shift the melt index after 3 extrusion cycles. Reclaim streams containing such ionomer films are limited below 2 wt% of the total blend.
Adhesive-free surface protection films based on DOWLEX 2071 are produced as 30–50 µm cast films with a low-polarity skin that forms temporary adhesion to polished steel, anodised aluminium, and glass. The film is not formulated with a pressure-sensitive adhesive; initial tack is derived from surface roughness, film stiffness, and the coefficient of friction of the sealant skin. Peel force is measured by 180° peel at 300 mm/min following a dwell time of 24 h at 23 °C; values between 0.2 N/25 mm and 1.5 N/25 mm are returned by typical structures. Higher peel force causes adhesive residue on sensitive cladding, while lower peel permits edge lifting during slitting and application. DOWLEX 2071 contributes stiffness and dimensional stability; casting film at 30–50 µm with a chill roll temperature of 20 °C limits post-extrusion shrinkage. Outdoor exposure of the film is not intended beyond 6–12 months, and UV-stabilised masterbatches are evaluated by ISO 4892-2 because unprotected DOWLEX 2071 film loses mechanical integrity after prolonged UV exposure. Under EU 1907/2006, the resin is supplied with a REACH registration; the final article condition is assigned after converting and does not require further authorisation for industrial packaging or building protection uses, but the converter remains responsible for documenting the article identity.
Die build-up from low-molecular-weight species is observed in the lip region after 8–12 h of continuous casting when the melt temperature exceeds 250 °C; periodic purging with a cast-grade LDPE reduces die-line formation. Screw speed on a 65 mm 30:1 L/D extruder at 120 kg/h is adjusted to maintain melt temperature below 240 °C.
Competitive Dow DOWLEX™ 2071 Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Among the DOWLEX linear low density polyethylene resins, DOWLEX™ 2071 is an ethylene-octene copolymer supplied in pellet form for thin-gauge flexible packaging. The nominal melt index is 2.3 g/10 min as determined by ASTM D1238 at 190 °C under a 2.16 kg load, and the nominal density is 0.920 g/cm³ as determined by ASTM D1505. The resin is manufactured by a solution polymerization process, which gives an essentially linear backbone with short-chain branches from octene-1 and negligible long-chain branching relative to autoclave low-density polyethylene. The chemical identity is polyethylene, CAS 9002-88-4. Suitability for blown film, cast film, and extrusion coating must be confirmed by line trials under production conditions; the datasheet values alone do not guarantee performance.
The following typical values are provided for material screening and are not to be interpreted as specification limits. Lot-to-lot variation is controlled within normal production tolerances.
| Property | Test Method | Typical Value |
|---|---|---|
| Nominal Density | ASTM D1505 | 0.920 g/cm³ |
| Melt Index | ASTM D1238, 190 °C, 2.16 kg | 2.3 g/10 min |
| Melting Temperature | ASTM D3418, differential scanning calorimetry | near 122 °C |
| Vicat Softening Temperature | ASTM D1525 | near 102 °C |
The melt index of 2.3 g/10 min places DOWLEX 2071 in the medium-flow LLDPE class. The density of 0.920 g/cm³ corresponds to a semicrystalline morphology with a melting endotherm typically near 122 °C. The Vicat softening temperature is typically near 102 °C under ASTM D1525. Load-bearing applications above 60 °C require creep data generated under the intended load and temperature; continuous service at elevated temperature is not established by a single Vicat value.
The density and comonomer chemistry define the solid-state morphology. Octene-1 branches are excluded from the crystal lattice, reducing lamellar thickness and increasing the amorphous tie-molecule population relative to butene-based LLDPE of the same density. This morphology contributes to the higher dart impact and tear resistance observed in film, but it also reduces flexural modulus compared with high-density polyethylene. Stiffness is evaluated by ASTM D790 or ISO 178, not inferred from density alone.
Because DOWLEX 2071 is produced by a solution process, the resin typically has a narrow molecular weight distribution and low gel content compared with some autoclave LDPE grades. Narrow molecular weight distribution reduces low-molecular-weight extractables and improves film-clarity stability, but it also reduces melt elasticity and can make the melt more sensitive to draw resonance in high-speed cast film. Draw resonance is controlled by optimizing the die-to-chill-roll air gap and by maintaining a stable melt curtain. Film haze is measured by ASTM D1003; clarity is measured by ASTM D1746 or equivalent.
Relative to a high-pressure LDPE of comparable melt index, DOWLEX 2071 has lower melt strength and lower melt tension because the solution-process backbone is essentially linear. On blown-film equipment this requires a die gap of 1.8 mm to 2.5 mm instead of the 0.8 mm to 1.2 mm die gap commonly used for LDPE. Bubble stability is maintained with a blow-up ratio of 2.0:1 to 2.5:1, whereas LDPE can be run at higher blow-up ratios. The benefit of the linear backbone is higher tensile strength and higher dart impact in the final film when measured by ASTM D882 and ASTM D1709 Method A.
Compared with a Ziegler-Natta butene LLDPE of the same density and melt index, the octene-1 comonomer in DOWLEX 2071 creates longer short-chain branches. Longer branches increase the probability of tie-chain formation between lamellae during film crystallization. The resulting film typically shows higher Elmendorf tear strength and higher dart impact at the same gauge. The difference is particularly relevant at film gauges below 25 µm; published data for this specific grade across all structures remain limited, and line trials are required to establish the actual property gain.
Within the DOWLEX family, DOWLEX 2071 differs from lower-melt-index grades such as DOWLEX 2045.09 by its higher melt index. The higher flow reduces extruder back pressure and enables thinner gauge drawdown on high-speed lines. Lower-melt-index grades are selected for heavy-gauge blown film where maximum dart impact and tensile strength are required at the expense of higher motor load and lower output.
On production-scale blown-film lines, DOWLEX 2071 is processed on single-screw extruders with 24:1 to 30:1 L/D barrier screws and Maddock mixing sections. The die is a spiral mandrel design with a die gap of 1.8 mm to 2.5 mm. A die gap below 1.5 mm raises die-lip shear stress and can trigger sharkskin melt fracture at lower output. Melt temperatures at the die are normally controlled between 190 °C and 230 °C. Extended residence time above 250 °C increases gel formation and should be avoided. The bubble is run at a blow-up ratio of 2.0:1 to 2.5:1, with frost-line height between 6 and 10 die diameters. Internal bubble cooling is used above approximately 80 kg/h on a 200 mm die to control bubble temperature. Air-ring air temperature is commonly 10 °C to 20 °C, and nip-roll temperature is kept at 15 °C to 25 °C to minimize blocking. Fluoropolymer-based polymer processing aids at active concentrations of 200 ppm to 500 ppm are added to suppress die-lip buildup and melt fracture. If melt fracture persists, the die gap is widened or output is reduced until the defect clears.
Blends with LDPE at 10% to 30% by weight are used when additional bubble stability is required. LDPE increases melt tension and lowers the risk of bubble flutter but can reduce dart impact compared with the unblended resin. The exact balance depends on die geometry and film gauge; no single ratio is universally valid.
For optical-grade film, die melt-temperature uniformity should be maintained within ±5 °C; wider variation creates draw resonance and haze bands. A gear melt pump or static mixer between the extruder and die reduces pressure pulsation and improves gauge uniformity. Field observations show that the most common processing failure is die-lip buildup, which appears as film streaks and width-gauge bands. It is caused by oxidation of polymer at the die lip and is managed with fluoropolymer process aids and periodic die cleaning. A second failure mode is bubble instability from too low a frost line or too high a blow-up ratio; this is corrected by raising the frost line to 6 to 10 die diameters and lowering BUR to 2.0:1 to 2.5:1.
Cast-film processing uses a flat-die extrusion line with a die gap of 0.4 mm to 0.8 mm and melt temperatures of 230 °C to 260 °C. The higher melt temperatures reduce viscosity and improve web uniformity, but residence above 280 °C is limited to avoid oxidative gel formation. A chill-roll temperature of 15 °C to 30 °C is maintained to control crystallinity and minimize blocking. Air-knife or vacuum-box edge pinning is required to reduce neck-in and edge beading. Line speeds above 200 m/min are common for thin-gauge cast film; at such speeds, melt curtain stability and gauge profile are controlled by die bolt adjustment and automatic profile control. Edge trim reclaim is added back into the extruder feed at ratios not exceeding 20% unless the line is equipped with a vented extruder and a melt filter.
In cast stretch film, DOWLEX 2071 is often blended with metallocene LLDPE at ratios from 70:30 to 50:50 to balance puncture resistance and stretch force. Published data for this specific grade in cast stretch-film blends are limited; film line trials are required to establish the optimum ratio. Cling performance is not provided by the base resin; tackifier-additive concentrates are required and must be selected for compatibility with the formulation.
For extrusion coating and lamination, DOWLEX 2071 can be processed at melt temperatures of 280 °C to 320 °C with an air gap of 150 mm to 250 mm. Compared with high-pressure LDPE, the melt curtain is less stable and requires a reduced air gap; neck-in is influenced by melt temperature and die-to-substrate distance. The resin is not a direct substitute for autoclave LDPE in high-speed coating without adjustment of the die gap, air gap, and melt temperature.
Heavy-duty shipping sacks, industrial liners, carrier bags, and agricultural films are typical applications for DOWLEX 2071. Film gauge is typically 75 µm to 150 µm for heavy-duty sacks. Mechanical properties of finished film are evaluated using ASTM D1709 Method A for dart impact, ASTM D1922 for Elmendorf tear, and ASTM D882 for tensile properties. For agricultural film, UV stabilization with hindered amine light stabilizers is mandatory; unstabilized polyethylene film embrittles under ASTM G154 cycling after a period that depends on geographic UV dose and film thickness. The resin is not a stand-alone UV-resistant grade.
For heat-seal applications, seal initiation temperature is measured by ASTM F88 or ASTM F1921. The octene-1 comonomer lowers seal initiation temperature relative to butene-based LLDPE of the same density. In form-fill-seal operations, seal settings of 100 °C to 120 °C with a dwell time of 0.5 s to 1.0 s and a seal pressure of 0.3 MPa to 0.5 MPa are typical starting points, but actual conditions must be established on the packaging machine because jaw design and film slip affect heat transfer.
The base stabilization package is intended for general-purpose film extrusion. If the resin is used in applications requiring long-term thermal aging or outdoor exposure, additional stabilizers must be compounded into the film. The choice of stabilizer affects food-contact compliance and odor; thioester antioxidants can generate odor in some low-density films and must be evaluated by organoleptic testing according to ISO 13302 or equivalent.
Because DOWLEX 2071 is a polyethylene copolymer composed of ethylene and octene-1, it falls within the class of olefin polymers described in 21 CFR 177.1520. Food-contact compliance is not granted by resin composition alone; the finished article must comply with extractive limits and end-use specifications in 21 CFR 177.1520(b) and 21 CFR 177.1520(c). In the European Union, the base polymer is subject to Regulation (EU) No 10/2011, including overall migration limits of 10 mg/dm² for general food contact and 60 mg/kg for infant food contact. The resin is not classified as hazardous under CLP Regulation (EC) No 1272/2008 in pellet form.
| Regulation | Status |
|---|---|
| 21 CFR 177.1520 | Olefin polymer class; final article testing required |
| Regulation (EU) No 10/2011 | Polyethylene polymer for food-contact plastics; overall migration limits apply |
| REACH | Polymer exempt from registration; ethylene and octene-1 monomers registered |
| RoHS Directive 2011/65/EU | No intentionally added lead, cadmium, mercury, hexavalent chromium, PBB, or PBDE |
Pre-drying is not normally required for DOWLEX 2071 because polyethylene is not hygroscopic. If condensation is present after cold storage, a dehumidified hopper dryer at 70 °C to 80 °C for 1 h to 2 h is sufficient. Melt temperatures above 300 °C must be avoided; prolonged hold-up above 250 °C causes oxidative degradation, gel defects, and off-color. The resin should not be blended with strong oxidizing agents or chlorinated polymers under high-temperature processing. Reclaim streams containing polypropylene or PET should be limited to 2% or less because of incompatibility and film appearance defects. Store in a closed, dry location at temperatures below 50 °C and away from direct sunlight. If antistatic or antifog additives are required, the final film must be re-evaluated for regulatory compliance.
As a non-polar polyolefin, DOWLEX 2071 is compatible with standard polyethylene film recycling streams. It can be re-extruded in post-industrial scrap systems if the scrap is free of paper labels, adhesive, and high-density contaminants. The amount of reclaim that can be reintroduced without loss of dart impact is machine-dependent; a starting range of 5% to 15% post-industrial scrap is common, but final properties must be verified by ASTM D4272 or ASTM D1709.