| HS Code | 271431 |
| Resin Type | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Octene |
| Density | 0.919 g/cm³ |
| Melt Index | 0.80 g/10 min |
| Melt Flow Ratio I10 I2 | 8.0 |
| Tensile Strength At Yield Md | 10.3 MPa |
| Tensile Strength At Yield Td | 10.3 MPa |
| Tensile Strength At Break Md | 30.3 MPa |
| Tensile Strength At Break Td | 25.5 MPa |
| Elongation At Break Md | 700% |
| Elongation At Break Td | 800% |
| 1 Secant Modulus Md | 190 MPa |
| 1 Secant Modulus Td | 210 MPa |
| Dart Drop Impact | 120 g |
| Elmendorf Tear Strength Md | 240 g |
| Elmendorf Tear Strength Td | 320 g |
| Haze | 11% |
| Gloss 45 | 75 |
| Vicat Softening Point | 100°C |
| Melting Point | 122°C |
| Crystallization Temperature | 105°C |
As an accredited Dow DNDA-8335 NT 7 Linear Low Density Polyethylene Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Dow DNDA-8335 NT 7 is supplied in 25 kg polyethylene bags, palletized and stretch-wrapped for secure transport and storage. |
| Container Loading (20′ FCL) | 20′ FCL loading of Dow DNDA-8335 NT 7 Linear Low Density Polyethylene Resin in 25 kg bags, palletized and secured. |
| Shipping | Dow DNDA-8335 NT 7 Linear Low Density Polyethylene Resin is a non-hazardous plastic resin, not regulated for transportation. Ship in 25 kg polyethylene bags, 1,000 kg bulk bags, or bulk containers. Keep dry and avoid heat, sparks, and open flames. Secure loads during transport. |
| Storage | Store in a cool, dry, well-ventilated area away from direct sunlight, heat, flames, and oxidizing agents. Keep original bags or containers closed and clean to prevent moisture and contamination. Stack pallets securely, avoid excessive height, ensure good housekeeping, and label containers clearly. Avoid dust generation and static discharge. Follow the manufacturer’s SDS and use appropriate PPE when handling. |
| Shelf Life | Two years from date of manufacture when stored in original packaging at temperatures below 50°C (122°F) in a cool, dry area. |
Where a heavy-duty industrial sack requires a puncture-resistant inner ply in the 80–120 µm gauge band, DNDA-8335 NT 7 is processed on high-stalk blown-film equipment with a single-screw extruder at 24:1–30:1 L/D and a barrier-section compression ratio of 3.0:1–3.5:1, feeding a spiral mandrel die with 1.8–2.5 mm die gap. Barrel set points are maintained from 180–195°C in the feed zone to 215–230°C at the die, while melt temperature is held at 215–235°C to avoid oxidative gel formation and preserve dart drop resistance per ASTM D1709. Blow-up ratio is held at 2.0:1–2.5:1, and frost line height is positioned 600–900 mm above the die lip to balance machine-direction and transverse-direction Elmendorf tear values per ASTM D1922; frost-line positioning above this range increases transverse-direction orientation and reduces machine-direction tear resistance enough to cause sack splitting at fill spouts. Material compliance for industrial non-food sacks references ASTM D4976 for polyethylene extrusion material specifications, ISO 1133-1:2022 for melt mass-flow rate verification, and REACH (EC) No 1907/2006; packaging waste heavy-metal limits are checked under EU Directive 94/62/EC. Formulation addition: DNDA-8335 NT 7 can be used as the sole resin or let down with 10–25 wt% low-density polyethylene homopolymer to increase melt strength and dart drop at high blow-up ratio; 1–3 wt% synthetic silica antiblock masterbatch and 0.5–1.5 wt% erucamide slip masterbatch are added for openability, and a fluoropolymer processing aid at 200–500 ppm suppresses melt fracture at die-land shear rates above 400 s⁻¹. Internal bubble cooling and dual-lip air-ring temperatures of 15–25°C sustain output of 400–650 kg/h on a 1,600 mm die line. Terminal products include FIBC outlet liners, bulk chemical sacks, fertilizer bag inner plies, and steel-coil overwrap.
Draw resonance on a cast-film line is suppressed by blending 10–20 wt% LDPE or by selecting DNDA-8335 NT 7 as a low-neck-in component in a multilayer structure; the phenomenon appears as periodic thickness oscillation when the draw-down ratio exceeds melt strength, typically at casting speeds above 250 m/min depending on air-gap and chill-roll temperature. Processors run a 30:1 L/D single-screw extruder with feed throat temperature 180–195°C, barrel 210–240°C, and die temperature 235–245°C, feeding a 0.8–1.0 mm die gap; the air gap is adjusted between 50–200 mm, and the chill roll is held at 18–25°C to fix film crystallinity before winding. Compliance for cast film destined for lamination includes ISO 1133-1:2022 for incoming resin lot melt-flow-rate verification, ASTM D792 for density, ISO 6383-2 for tear resistance, and ASTM D882 for tensile modulus of the final film; if the film is used in food contact, FDA 21 CFR 177.1520(c) and EU Regulation (EU) No 10/2011 apply. Addition ratio: a fluoropolymer processing aid at 200–400 ppm is used to delay melt fracture, 5–15 wt% mLLDPE may be added to modify elongation at break, and 0.5–1.5 wt% antiblock concentrate is added only when the lamination film is wound in high-humidity conditions. Terminal products include BOPP/BOPET lamination base, metallised film base, hygiene overwrap, and surface-protection film.
After UV stabilisation is introduced at the feed throat, DNDA-8335 NT 7 is extruded into agricultural silage covers and greenhouse sheeting at thicknesses from 100 µm to 200 µm, using a high-stalk blown-film line with die temperature 205–225°C, blow-up ratio 2.0:1–2.5:1, and frost line height 500–800 mm. The stabilisation package is typically added at 2–6 wt% of a HALS/UV-absorber masterbatch with 20% active content, yielding final active HALS concentration in the 0.4–1.2 wt% range; published outdoor weathering data for DNDA-8335 NT 7 with this specific stabiliser package are limited, but general LLDPE agricultural film systems require a HALS concentration of 0.3–1.0 wt% active material to pass EN 13206:2017 accelerated aging criteria. Compliance for agricultural plastics references EN 13206:2017 for thermoplastic films used in agriculture and horticulture, ISO 527-3 for film tensile properties, and REACH (EC) No 1907/2006 for UV stabiliser registration; soil-biodegradable mulch film standards do not apply to conventional low-density PE. Formulation addition: 10–20 wt% LDPE is used to increase extensibility during bale wrapping, and 0.5–1.0 wt% anti-fog masterbatch may be added for greenhouse films to lower surface tension and reduce droplet formation. Terminal products include silage bale stretch covers, greenhouse side sheets, low-tunnel film, and temporary silo covers.
Coextrusion lines producing symmetrical three-layer and five-layer films use DNDA-8335 NT 7 as the food-contact sealant layer at 10–20 µm total layer gauge, with the barrier core of EVOH or polyamide and tie layers of anhydride-modified polyethylene. The resin is processed in the skin-layer extruder at barrel temperatures 180–220°C and die temperature 215–235°C, with a die gap of 2.0–2.5 mm; blow-up ratio is kept at 2.0:1–2.5:1 to match barrier-layer draw ratios and prevent interfacial instability. Food-contact compliance is verified under FDA 21 CFR 177.1520(c) for olefin polymers and EU Regulation (EU) No 10/2011, including overall migration limit 10 mg/dm² under the specified food simulants; specific migration limits for slip additives such as erucamide are checked under the corresponding EU positive list entries. Addition ratio: the sealant skin layer contains 0.5–1.5 wt% synthetic silica antiblock, 0.1–0.4 wt% slip additive masterbatch with 5–10% erucamide active content, and 200–400 ppm fluoropolymer processing aid in the first 24 h of a campaign; pre-drying is not required at ambient relative humidity below 60%, but condensation on pellets must be avoided because trapped moisture can produce surface splay and pinholes at thin gauges. Terminal products include frozen food pouches, dry-food side-gusset bags, coffee package inner liners, and lamination-grade sealant webs.
Elastic recovery after machine-direction orientation is determined by the ratio of DNDA-8335 NT 7 to octene-based mLLDPE; published data for this exact blend at 70–100 µm gauge on stretch-hood lines are limited, but industrial trials commonly use 20–40 wt% mLLDPE to raise dart impact and puncture resistance without sacrificing transverse-direction tear. The film is produced on cast-film lines with 30:1 L/D extruders and a die gap of 0.8–1.2 mm, air gap 50–120 mm, chill-roll temperature 15–20°C, and winding tension controlled within 50–100 N/m to prevent blocking. Compliance for pallet hoods includes ISO 527-3 for tensile properties, ISO 6383-2 for tear propagation, ASTM D5458-95(2012) for cling and peel force, and REACH (EC) No 1907/2006; where used in export packaging, ISPM 15 applies to the wooden pallet, not to the polyethylene hood. Addition ratio: 0.5–2.0 wt% cling masterbatch based on polyisobutylene or an alternative tackifier is added to the outer layer, 0.5–1.5 wt% slip masterbatch is added to the inner layer, and 200–500 ppm fluoropolymer processing aid is used when line speed exceeds 200 m/min. Terminal products include pallet hoods, cold-chain stack covers, and heavy-duty logistics overwrap.
In extrusion coating of paperboard and aluminium foil for liquid packaging, DNDA-8335 NT 7 is applied at a coating weight of 15–25 g/m² through a flat die onto a corona-treated substrate, using a 30:1 L/D extruder with barrel temperatures 210–240°C and die temperature 240–255°C; the melt curtain is drawn into a laminator nip at line speeds of 100–250 m/min, and the chill roll is held at 15–20°C to quench the polyethylene without excessive thermal stress at the substrate interface. Compliance for food-contact cartons includes FDA 21 CFR 177.1520(c), EU Regulation (EU) No 10/2011, and ISO 1133-1:2022 for lot-to-lot melt-flow verification; converters also test peel strength to aluminium under ASTM D1876 or seal strength under ASTM F904. Addition ratio: 10–20 wt% LDPE is added to improve neck-in control and draw-down stability, 0.5–1.5 wt% antiblock masterbatch is included only where the coated reel is stored beyond 30 days at ambient humidity, and 300–500 ppm fluoropolymer processing aid is added to avoid die-lip deposit. Terminal products include liquid carton sealant layers, paperboard sachets, retort-free stand-up pouch bases, and aluminium foil insulation facings.
Competitive Dow DNDA-8335 NT 7 Linear Low Density Polyethylene Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Dow DNDA-8335 NT 7 Linear Low Density Polyethylene Resin is a pelletized, low-pressure polymerized ethylene copolymer supplied with a natural stabilizer package. The grade is intended for thin-gauge extrusion and injection-molding operations in which elevated melt flow must be balanced against adequate melt strength and toughness. Manufacturer technical documentation identifies the nominal melt flow rate as 5.0 g/10 min at 190 °C/2.16 kg using ASTM D1238 or ISO 1133-1, and the nominal density as 0.926 g/cm³ using ASTM D1505 or ISO 1183-1. Lot-specific values may differ by production campaign and must be confirmed against the certificate of analysis. The resin belongs to the linear low-density polyethylene class, meaning the backbone is essentially linear and short-chain branching is introduced catalytically rather than by high-pressure radical polymerization.
| Property | Representative value | Test method |
| Melt flow rate | 5.0 g/10 min at 190 °C/2.16 kg | ASTM D1238, ISO 1133-1 |
| Density | 0.926 g/cm³ | ASTM D1505, ISO 1183-1 |
| Tensile stress at yield | 12.0 MPa | ASTM D638, Type IV at 50 mm/min |
| Ultimate tensile stress | 20.0 MPa | ASTM D638 |
| Elongation at break | 800% | ASTM D638 |
| Flexural modulus | 0.30 GPa | ASTM D790 |
| Vicat softening point | 102 °C | ASTM D1525, Rate A |
| Melting temperature by DSC | 122 °C | ISO 11357-3 |
The data above are compiled from published manufacturer literature and normalized to standard test methods. They represent a starting point for material selection, not an end-use specification. Differences in sample preparation, thermal history, and conditioning can shift measured values by several percent. Published data for this specific configuration are limited where multi-axial impact and hot-tack testing are concerned; those properties should be evaluated on production film or molded parts before final qualification.
The primary structural difference between high-pressure low-density polyethylene and this linear low-density grade is the absence of long-chain branching. High-pressure LDPE possesses a branched architecture that contributes to high melt elasticity, pronounced shear thinning, and stable bubble formation in blown film. Dow DNDA-8335 NT 7, by contrast, derives its processability from controlled short-chain branching along a linear backbone. This produces a higher ultimate tensile stress and higher elongation at break than a high-pressure LDPE of equivalent melt flow rate when compared under ASTM D638. The lower degree of long-chain branching also raises the onset of melt fracture; therefore, cast-film lines and extrusion-coating dies may run at higher throughput before sharkskin or draw resonance appears.
In practice, the differences are visible in dart drop impact ASTM D1709 and Elmendorf tear ASTM D1922. Linear low-density polyethylene grades of this type typically show greater puncture and tear resistance than high-pressure LDPE at the same gauge, permitting down-gauging in heavy-duty sacks and industrial liners. The trade-off is optical: high-pressure LDPE generally produces lower haze and higher gloss in blown film because of its lower crystalline orientation and smoother surface morphology. This grade therefore tends to be selected when mechanical toughness is the primary requirement and clarity is secondary. For applications requiring both clarity and toughness, blending or coextrusion with a high-clarity layer is common.
Rheologically, the resin exhibits a narrower molecular weight distribution and a more Newtonian plateau at low shear rates than high-pressure LDPE. Screw torque and melt pressure in a single-screw extruder with a barrier screw and an L/D ratio of 24:1 are therefore influenced more strongly by temperature set points than by shear adjustment. Melt temperature should be maintained between 220 °C and 260 °C to avoid excessive pressure at the die inlet. The higher melting point relative to high-pressure LDPE also permits higher sealing temperatures, but seal initiation may be slightly higher than for a lower-density LDPE grade. The selection of comonomer type, which is controlled by the manufacturer and documented in the product specification, affects hot-tack and seal-initiation behavior and should not be assumed from density values alone.
In extrusion coating, differences from high-pressure LDPE are readily observable in neck-in and draw-down. High-pressure LDPE is often added to linear low-density polyethylene coating formulations to reduce neck-in and stabilize the melt curtain. Running this grade as the sole coating resin may produce a wider neck-in at a given die width unless processing conditions are adjusted. Typical adjustments include reducing the air gap, increasing chill-roll speed, or using a die with a narrower deckle. The resin should be tested on the target coating line with a draw ratio appropriate for the substrate because published data for this specific configuration is limited.
In extrusion coating and lamination, the material is commonly processed through a polyolefin screw with a length-to-diameter ratio of at least 24:1 and a compression ratio between 2.5:1 and 3.5:1. Barrel temperatures are ramped from 180 °C at the feed throat to 250–260 °C at the adapter and die. The die gap is usually set between 0.5 mm and 0.8 mm for coating weights below 30 g/m². Chill-roll surface temperature is held between 15 °C and 30 °C to solidify the web and control crystallinity. Higher chill-roll temperatures reduce thermal shock and improve adhesion to porous substrates but may increase blocking tendency at winding. Processing experience on production-scale extrusion coaters shows that melt curtain stability can be optimized by an air gap shorter than 150 mm for this melt index class. Operators should monitor edge trim generation and web tension because the linear backbone produces a higher melt tension than a comparable high-pressure LDPE at the same melt temperature.In cast-film production, the resin is extruded through a flat die and quenched on a water-cooled or oil-cooled chill roll. The high melt flow rate supports thin-gauge output, but die-lip cleanliness and uniform melt distribution are critical. A coat-hanger die with a die gap of 0.5 mm to 0.7 mm is standard for gauges between 15 µm and 50 µm. Melt temperature is usually held between 240 °C and 260 °C to eliminate low-flow-induced melt fracture and to maintain acceptable draw. Draw resonance, which appears as a periodic oscillation in film thickness and tension, tends to be more pronounced with linear low-density polyethylene than with high-pressure LDPE because of the reduced strain-hardening behavior. Its onset is a function of draw ratio, air gap, chill-roll speed, and melt temperature. Increasing melt temperature or reducing the air gap to below 100 mm can shift the critical draw ratio upward.
Chill-roll chemistry and surface roughness influence the quench rate and thus the crystalline morphology. A polished, chromium-plated roll with a surface roughness Ra below 0.05 µm is used when high gloss and low haze are required. A matte roll or an air knife is used when the film must be wound without blocking. If the film is stretched in the machine direction after quenching, the cast web must be reheated to 80–100 °C before the orientation rolls. Machine-direction orientation at ratios below 5:1 is typical for high-strength overwrap and label film, but the exact ratio depends on the required machine-direction tensile modulus and tear balance. The higher melting point and stiffer crystalline phase of this grade relative to many high-pressure LDPE grades reduce the thermal shrinkage of the final film at temperatures below 70 °C.
The resin is not hygroscopic to the extent of polyamide or polyester, but surface moisture from condensation can create surface defects on cast film. If storage has occurred in an environment where relative humidity exceeds 60% and the pellet surface is cold, pre-drying at 70–80 °C for 2–4 h should be performed before extrusion. This is an operational boundary rather than a standard requirement for the polymer chemistry. Failure to remove surface moisture can result in bubbles, pinholes, or visible moisture splay in the cast web. The material should not be dried at temperatures above 90 °C for extended periods because pellet agglomeration may occur in hopper dryers without adequate air mixing.
Blending this product with post-industrial or post-consumer polyethylene streams can reduce cost, but the final melt flow rate and density shift according to the blend ratio. A recycled linear low-density polyethylene stream with a melt flow rate of 2.0 g/10 min and a density of 0.920 g/cm³ will reduce overall melt flow and slightly reduce stiffness when blended at 20–30 wt%. The effect on the processing window is not linear because polyethylene blends can exhibit co-continuous crystalline phases and differing nucleation behavior. A twin-screw extruder with a screw L/D ratio of 40:1 and dispersive mixing elements provides better homogenization than a single-screw dry blend. Melt filtration through a screen pack of 100–200 mesh is recommended when recycled content is introduced, because gel contamination and metal fines from the waste stream can cause die-lip build-up and film defects.
The blend ratio should be confirmed by melt flow testing under ASTM D1238 and density testing under ASTM D1505 on the compounded pellet and on the final film. A batch-to-batch variance in recycled content of 5 wt% can shift the film gauge distribution and alter the Elmendorf tear balance in oriented films. For cast-film operations, a screening study on a pilot line with a chill-roll speed range of 20–60 m/min is advisable before plant-scale implementation. This avoids the production-scale failure mode in which unstable melt curtains generate edge fold-over and automatic gauge-control oscillation during continuous winding.
When this grade is used in thin-wall injection molding, the higher melt flow allows filling of multi-cavity tools at moderate injection pressures, but the semi-crystalline solidification behavior requires tighter temperature control than amorphous thermoplastics. Barrel temperatures should be profiled from 190 °C near the feed to 230 °C at the nozzle. Mold surface temperature should be controlled between 10 °C and 30 °C to achieve acceptable cycle time. Demolding of polyethylene is generally easier than with polypropylene of the same flow length because the lower modulus reduces ejection drag, but the part must be sufficiently crystallized to prevent post-demolding warpage. The clamp force requirement for a given projected area is lower than for a filled polypropylene because polyolefin cavity pressures are typically below 40 MPa at the gate during the packing phase.
Mold shrinkage for low-density ethylene copolymers of this density band is typically in the range of 1.5% to 2.0%, with the higher value in the flow direction and the lower value transverse to flow. This anisotropy is a processing variable rather than a material constant; it depends on gate position, packing pressure, and cooling rate. For lids, closures, and thin-walled containers, the shrinkage range must be confirmed with a cavity-pressure sensor and a short-shot study on the production tool. The material should not be assumed to replicate the shrinkage of a high-pressure LDPE of equal melt index because the higher ultimate elongation and different crystallization behavior produce a different residual stress pattern.
Incompatibility concerns are relatively low for non-polar polyolefins, but the resin should not be blended with polar barrier polymers such as polyamide or ethylene vinyl alcohol without a tie-layer because interfacial adhesion is insufficient and layer delamination occurs under flexural stress. Printability and adhesion require corona or plasma treatment for film and surface treatments for molded parts. The oxidative induction time of the natural grade is appropriate for normal processing at the temperatures specified above, but prolonged hold-up at temperatures above 280 °C may deplete the stabilizer package and produce discoloration or odor. During purging, a low-melt-index polyethylene purge compound should be used before shut-down to minimize black specks from polymer degradation in hot runners.
The material is supplied as natural pellets and should be stored in a dry, covered area at ambient temperatures below 50 °C. Ultraviolet exposure over multiple weeks can reduce stabilizer performance and initiate surface oxidation. Bulk-railcar deliveries and silo storage should be sampled according to ISO 9001 material-handling procedures to ensure that pellet fines do not exceed a level that affects downstream feeding consistency. Because the resin is a thermoplastic, reprocessed material from clean edge trim or rejected pre-consumer parts can be reintroduced within the producer’s recommended recycle ratio if the material has not been degraded by multiple heat histories.
| Regulatory reference | Scope | Verification requirement |
| FDA 21 CFR 177.1520 | Olefin polymers in food-contact articles | End-use conditions, thickness, and food-simulant migration must be verified for the final article. |
| Regulation (EU) 10/2011 | Plastic materials and articles intended to contact food | Migration testing under worst-case time and temperature is required before a final compliance declaration. |
| REACH (EC 1907/2006) | Registration, evaluation, and authorization of chemicals in the European Union | Supplier safety data sheet and substance registration dossiers should be consulted for substance identity and use restrictions. |
| Directive 2011/65/EU | Restriction of hazardous substances in electrical and electronic equipment | Applicable only if the resin is incorporated into an electrical or electronic product subject to the directive. |
The compliance table above is not a blanket certification. Each application must be assessed against the full text of the regulation, including any amendments and national implementations. For medical packaging or pharmaceutical closures, additional testing such as USP Class VI or ISO 10993 biocompatibility may be required, and published data for this grade in those specific configurations should be obtained from the manufacturer or qualified testing laboratory.