| HS Code | 981345 |
| Polymer Type | Anhydride-modified linear low-density polyethylene |
| Functional Group | Maleic anhydride |
| Carrier Resin | Linear low-density polyethylene |
| Physical Form | Pellets |
| Density | 0.920 g/cm³ |
| Melt Index | 2.5 g/10 min at 190°C/2.16 kg |
| Melting Point | 123°C |
| Vicat Softening Point | 95°C |
| Tensile Strength At Break | 15 MPa |
| Elongation At Break | 600% |
| Flexural Modulus | 250 MPa |
| Shore D Hardness | 50 |
| Recommended Processing Temperature | 200-260°C |
| Adhesion To Evoh | Excellent |
| Adhesion To Nylon | Excellent |
| Adhesion To Metal | Excellent |
As an accredited Dow Bynel® 41E871 Anhydride Modified LLDPE factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaging: 25 kg polyethylene bags of Dow Bynel® 41E871, 40 bags (1,000 kg) per pallet. |
| Container Loading (20′ FCL) | 20′ FCL container loading: Dow Bynel® 41E871 Anhydride Modified LLDPE, properly palletized and securely stowed for safe, efficient sea transport. |
| Shipping | Dow Bynel 41E871 Anhydride Modified LLDPE is shipped as non-hazardous, solid polymer pellets in moisture-resistant bags, boxes, or bulk totes. It is not regulated for DOT, IMDG, or IATA transport, requiring no UN number, hazard class, or placards. Store dry, away from excessive heat. |
| Storage | Store Dow Bynel 41E871 in original, tightly closed packaging in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, flames, and strong oxidizers. Protect from moisture, dust, and contamination. Avoid temperatures above 40–50°C. Keep separate from food, feed, and incompatible materials. Rotate stock and use within the supplier’s recommended shelf life. Pre-dry if specified before processing. |
| Shelf Life | Typically 24 months from manufacture when stored unopened in cool, dry conditions, away from direct sunlight and moisture. |
In five-layer cast coextrusion lines producing nylon- or EVOH-containing barrier film for vacuum skin packaging, Bynel® 41E871 is metered into the two adhesive sublayers between the polyolefin skins and the barrier core. The resin has a melt flow rate near 2.5 g/10 min under ISO 1133-1 at 190 °C/2.16 kg and density near 0.91 g/cm³, which places it below the viscosity of typical LDPE tie resins and permits thin-gauge application without excessive die lip pressure. The typical layer distribution for a 120 µm total film is 28 µm LLDPE skin, 8 µm Bynel® 41E871, 10 µm EVOH with 38 mol% ethylene, 8 µm Bynel® 41E871, and 66 µm LLDPE sealant. Barrel zones for the tie resin are set at 170 °C to 210 °C, while the die body is held at 215 °C to 225 °C; this keeps the grafted anhydride below the threshold where gel specks become visible. On a 1,200 mm cast die with a 0.65 mm die gap, the tie-layer melt curtain remains stable down to 5 µm gauge, but below 4 µm the film exhibits oscillating thickness variation across the web due to inconsistent melt bank filling. Peel adhesion is measured in accordance with ASTM F904-16 using 25.4 mm wide strips and a crosshead speed of 254 mm/min; migration of failure from interfacial delamination to LLDPE film yielding occurs when the tie layer reaches 12–15 µm. Processors report that adhesion to EVOH is degraded if the tie resin remains in the adapter above 240 °C for more than 8 minutes, because extended residence time accelerates crosslinking and raises melt pressure. Purge with fractional-melt LLDPE between campaigns is standard. Under U.S. food-contact evaluation, the structure is generally assessed under 21 CFR 175.105 for adhesive layers and 21 CFR 177.1520 for the olefinic base resin, while EU compliance follows Regulation (EU) No 10/2011 with overall migration limited to 10 mg/dm² for the finished laminate. End products include formable vacuum packages for processed meat, cheese, and case-ready red meat where the tie layer must retain adhesion through thermoforming at 90–110 °C and subsequent cold-storage flexing.
| Standard / Regulation | Scope | Relevant Parameter |
|---|---|---|
| 21 CFR 175.105 | Adhesives used in food-contact articles | Extractive limits under conditions of use |
| 21 CFR 177.1520 | Olefin polymers in food-contact articles | Density, maximum extractable fraction |
| Regulation (EU) No 10/2011 | Plastic materials and articles for food contact | Overall migration limit 10 mg/dm² |
| ISO 1133-1:2022 | Melt mass-flow rate determination | 190 °C, 2.16 kg |
| ASTM F904-16 | T-peel for flexible laminates | 25.4 mm width, 254 mm/min |
Extrusion lamination of aluminium foil to LLDPE sealant films for retortable stand-up pouches uses Bynel® 41E871 as the molten adhesive web between foil and polyolefin backing. The coating weight is typically 8–20 g/m², with the lower end used for dry food lidding and the upper end for aggressive retort cycles at 121 °C for 30 min. Melt temperature at the T-slot die is maintained at 285–310 °C to generate controlled surface oxidation, which promotes carboxylic acid interaction with the aluminium oxide layer; below 265 °C, peel strength to foil becomes erratic, while above 320 °C the web smokes and edge-lift defects increase. The air gap is set between 120 mm and 180 mm, and ozone addition is applied in the melt curtain at the air gap, with generator output adjusted until web neck-in across a 1,200 mm die is held below 20 mm; published data for this specific grade and ozone generator configuration is limited. Adhesion is evaluated after 24 h conditioning at 23 ± 2 °C and 50 ± 5 % relative humidity using ASTM F904-16; acceptable values for aluminium-to-LLDPE bonds are typically reported in the range 3–6 N/25 mm, but converters should establish internal limits against their specific foil temper and sealant additive package. The final laminate structure is used for retortable food pouches, pharmaceutical sachets, and fibrous insulation facings, where the anhydride tie layer must withstand both steam retort and post-retort flex cracking.
For factory-applied three-layer polyethylene pipeline coatings, Bynel® 41E871 functions as the intermediate adhesive layer between the fusion-bonded epoxy primer and the extruded HDPE topcoat. The steel pipe is first grit-blasted to Sa 2½ in accordance with ISO 8501-1, then inductively heated to 170–200 °C. Fusion-bonded epoxy powder is electrostatically deposited at 80–150 µm and must remain in its gel window when the tie layer is applied; if the pipe surface drops below 150 °C, the grafted anhydride does not wet the partially cured epoxy, and if it exceeds 210 °C, the fusion-bonded epoxy undergoes rapid advancement and adhesive interdiffusion is lost. The Bynel® 41E871 layer is extruded at 220–240 °C through a sheet die and applied in a single spiral wrap at 170–250 µm. Because the resin is LLDPE-based with density near 0.91 g/cm³, the tie layer remains flexible after application, which reduces disbonding at field bends where HDPE topcoats fail in flexure. The outer topcoat is applied simultaneously at 2.5–3.7 mm using a separate side-fed extruder, and the final system is water-quenched after a 20–40 s lay-flat window. Adhesion is tested under the peel test provisions of ISO 21809-1:2018 using 25 mm wide strips at 20 ± 2 °C; destructive peel should show cohesive failure in the tie layer rather than clean separation at the fusion-bonded epoxy interface. Compliance documentation is maintained against DIN 30670 for three-layer PE coatings and ISO 21809-1 for petroleum and natural gas industries; imported lots are accompanied by lot-specific melt flow rate under ISO 1133-1:2022 at 190 °C/2.16 kg and density under ISO 1183-1. End products are transmission pipelines, water-injection flowlines, and offshore riser anti-corrosion coatings, where the tie layer must tolerate cathodic disbondment conditions and thermal cycling from −40 °C to +85 °C.
High-density filler masterbatches for extrusion coatings and rigid sheet are produced with Bynel® 41E871 gravimetrically metered at 2–6 wt% of the compound to improve interfacial wetting of calcium carbonate or talc within an LLDPE/LDPE carrier. Compounding is performed on a co-rotating twin-screw extruder with 40:1 L/D, barrel temperatures from 150 °C in zone 1 to 200 °C at the die, and atmospheric vacuum venting after a side-fed mineral addition at 60–70 wt% filler loading. The anhydride functionality reacts with free hydroxyl groups on the mineral surface, but published data for this specific Bynel® grade at filler loadings above 70 wt% is limited; compounders therefore run screening trials at 2 wt%, 4 wt%, and 6 wt% to map torque and melt pressure before large-scale use. Torque typically drops 5–15 % compared with an unmodified LLDPE carrier at equal filler content, and extrudate surface roughness is reduced, but the effect depends on particle size distribution and surface moisture. The compounded pellets are used in breathable film concentrate let-down at 10–30 %, where the final film contains 20–50 wt% calcium carbonate and is converted into hygiene backsheet, surgical drape, and construction vapour-barrier applications. REACH registration is required for EU supply, and the product is routinely screened against RoHS Directive 2011/65/EU for Pb, Hg, Cd, Cr(VI), PBB, and PBDE when used in electronic packaging applications.
When coextruding six-layer barrier bottles for agricultural chemical and solvent-based cleaner containers, Bynel® 41E871 is extruded between HDPE skins and an EVOH or polyamide barrier core. The layer distribution is typically 1.5–3.0 wt% tie resin per adhesive layer and 2.0–4.0 wt% EVOH in the finished article, with the balance consisting of high-molecular-weight HDPE. Barrel temperatures for the tie extruder are maintained between 175 °C and 205 °C, while the multi-layer die head is set at 200–215 °C to balance parison swell and layer uniformity. Melt strength of the LLDPE-based tie is lower than that of the HDPE skins, so a parison die gap above 1.2 mm can create local tie-layer thinning at the pinch-off weld; bottles with pinched-off tail flash are therefore sectioned and examined by polarized light microscopy at 200× to verify that the tie layer does not disappear within 2 mm of the weld line. Drop impact resistance of filled bottles is evaluated according to UN Manual of Tests and Criteria Part I for dangerous goods packaging, and chemical resistance is confirmed by storing filled containers at 40 °C for 21 days with no visible delamination. The final applications include multilayer HDPE containers for hydrocarbon-based degreasers, agricultural emulsifiable concentrates, and industrial adhesives, where solvent permeation through the polar barrier must remain below regulatory thresholds for volatile organic compound emissions. For U.S. shipments, the finished package may be evaluated under 49 CFR 178.603 performance tests when exceeding 1.2 L, while EU supply requires a packaging safety assessment under Regulation (EC) No 1272/2008 for classification and labelling of the filled contents.
Coextrusion coating of liquid packaging board for gable-top and aseptic cartons uses Bynel® 41E871 as the interior tie layer between paperboard and aluminium foil or between foil and the LLDPE heat-seal layer. The resin is coextruded at 12–20 g/m² with a low-density LDPE skin through a flat die onto the moving paperboard web at line speeds of 180–360 m/min. Melt temperature at the die ranges from 270 °C to 300 °C to ensure oxidation and adhesion to the paperboard surface, but residence time in the die lip must be kept below 5 minutes because LLDPE-based grafts begin to form gel-like crosslinked particles under extended shear at high temperature. Chill roll temperature is set between 12 °C and 18 °C to quench the laminate and prevent backside curl. The tie layer must survive downstream creasing and folding at 2–4 mm radius without cracking, and adhesion is tested by peeling the foil from the paperboard after 1 h water contact at room temperature. The final cartons are used for UHT milk, juice, and liquid food service applications; the food-contact status of the laminated board is assessed under 21 CFR 176.170 for paper and paperboard components, while the extruded adhesive layer is covered by 21 CFR 175.105. Published data for 41E871 in aseptic carton structures is limited, so converters validate peel strength and water immersion resistance on their specific board stock.
Competitive Dow Bynel® 41E871 Anhydride Modified LLDPE prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Dow Bynel® 41E871 is an anhydride-modified linear low-density polyethylene resin supplied as translucent pellets. The grade designation 41E871 identifies an LLDPE backbone carrying anhydride functionality for reactive melt-phase adhesion. The material is specified as a tie-layer resin in coextruded films, sheet, blow-molded containers, and pipe coatings where polyolefin layers must be bonded to polar barrier resins or metals. Unlike unmodified LLDPE, Bynel 41E871 does not rely solely on mechanical interlock; it forms covalent linkages at the interface with polyamide and EVOH under normal melt processing. The absence of free acid groups and the low moisture absorption of the polyethylene backbone distinguish it from ethylene-acrylic acid copolymers and from ionomers.
The adhesion generated by Bynel 41E871 depends on interfacial temperature, contact time, and polar end-group availability. In coextruded blown film, the tie layer commonly exits the die at 220°C to 250°C; at lower melt temperatures, imide or ester bond formation with polyamide or EVOH is incomplete. Equipment with inadequate screw mixing can produce an unreacted boundary layer thicker than 10 µm. Peel adhesion tested according to ASTM F904 on polyamide/tie/PE laminates often shows cohesive failure within the polyolefin layer rather than adhesive failure, provided melt contact is maintained for adequate time. Published numerical peel strength data for Bynel 41E871 on all substrate grades is limited; therefore, line-specific trials are necessary.
Moisture management in the barrier layer controls process stability. Polyamide and EVOH absorb water; when polyamide pellets exceed 0.2% moisture by Karl Fischer titration according to ISO 15512, hydrolysis at the interface produces voids and reduces peel strength. Bynel 41E871 itself is hydrophobic, with water absorption below 0.05% at 23°C and 50% relative humidity when measured by ASTM D570. Drying of the tie layer is unnecessary unless contaminated regrind is introduced. Multi-layer dies with 30:1 L/D single-screw extruders running at screw speeds from 30 min⁻¹ to 90 min⁻¹ provide adequate plastication; higher speeds increase shear heating and raise melt temperature.
Typical properties are determined under standard conditions. The melt flow rate is measured at 190°C under 2.16 kg load according to ASTM D1238; density is measured by ASTM D1505; melting point and crystallization are characterized by differential scanning calorimetry per ASTM D3418. The following supplier-published typical data should be confirmed against the certificate of analysis for each lot.
| Property | Test Method | Typical Value |
|---|---|---|
| Melt flow rate | ASTM D1238 (190°C/2.16 kg) | 2.0–3.5 g/10 min |
| Density | ASTM D1505 | 0.905–0.920 g/cm³ |
| Melting point | ASTM D3418 | 120–125°C |
| Vicat softening point | ASTM D1525 | 85–100°C |
| Tensile strength at break | ASTM D638 | 10–15 MPa |
| Elongation at break | ASTM D638 | 700–900% |
Bynel 41E871 is characterized by linear polyethylene crystallization behavior and does not require the same acid-corrosion-resistant screws as ionomer or acid copolymer processes. Extrusion melt temperatures from 200°C to 260°C are typical. At barrel settings above 280°C, the polyethylene backbone may undergo oxidative chain scission, producing gel particles and discoloration; purge with a low-melt-index polyolefin is recommended before shutdown. In cast film, chill-roll temperatures from 15°C to 30°C are used to stabilize the web. The anhydride functionality can hydrolyze if stored open in high humidity; sealed bags should be kept below 50°C and protected from direct sunlight.
In a five-layer cast film line with two barrier layers, replacing a non-functional LLDPE skin layer with Bynel 41E871 changes adhesion but not the draw resonance behavior significantly. The resin has similar draw-down characteristics to LLDPE, but its melt elasticity may be slightly lower; die lip build-up can occur if the extruder barrel is not purged of oxidized PP or HDPE. Interfacial instability appears as visible wavy lines at the tie/EVA interface under high line speeds. Use of a 250 mm slot die with 0.5–0.8 mm die gap and 30 m/min to 100 m/min line speed is representative of production-scale behavior. Published data for this specific configuration is limited.
Food-contact suitability is not determined solely by the base resin. Compliance statements should be confirmed through supplier documentation. Typical food-contact status is governed by regional approvals, including FDA 21 CFR 177.1520 for olefin polymers when the product meets applicable extractive limits. EU compliance may require verification under Regulation (EU) No 10/2011 and its amendments. Because Bynel 41E871 contains reactive anhydride functionality, the final article must be evaluated for overall migration under EU 10/2011 test conditions specific to the food simulant and time-temperature profile. Published data for this specific configuration is limited.
The product is selected for coextruded barrier film used in food packaging, where EVOH or polyamide provides oxygen barrier and Bynel 41E871 prevents delamination. In a three-layer PA/tie/PE film, peel strength after 72 h at 23°C is typically higher than the same structure without a tie layer. Adhesion to EVOH depends on ethylene content; EVOH grades with 44 mol% ethylene and below are more difficult to bond if melt temperature is under 210°C. Adhesion to polyamide is influenced by amine end group concentration. Aminopropylsilane-treated polyamides may reduce required tie-layer thickness, but the anhydride functionality can react prematurely with amine-based additives.
Relative to a maleic anhydride grafted high-density polyethylene, Bynel 41E871 has a lower flexural modulus and improved cold-temperature impact retention. Relative to an unmodified LLDPE, it increases peel adhesion without adding measurable oxygen permeability. Relative to an ethylene-acrylic acid copolymer, the anhydride-modified LLDPE is less corrosive to steel surfaces and does not require vented barrel extraction for free acid. However, Bynel 41E871 is not a direct replacement for silane-grafted moisture-crosslinking adhesives in hot-water pipe applications, where condensation cure dominates. The table compares generic tie-resin classes using standardized test designations where available.
| Tie-Resin Class | Adhesion Mechanism | Moisture Sensitivity | Typical Processing Range | Equipment Requirement |
|---|---|---|---|---|
| Bynel 41E871 anhydride-modified LLDPE | Covalent imide/ester bonds | Low | 200–260°C | Standard polyolefin screw |
| Maleic anhydride grafted HDPE | Covalent imide/ester bonds | Low | 210–275°C | Standard polyolefin screw |
| Ethylene-acrylic acid copolymer | Hydrogen/ionic bonding | Moderate | 180–230°C | Corrosion-resistant screw and barrel |
| Unmodified LLDPE | Mechanical interlock only | Low | 190–250°C | Standard polyolefin screw |
Operation outside the stated temperature ranges may produce interfacial defects, odor, or gel formation. The anhydride functionality is not compatible with uncontrolled amine-based additives, and prolonged contact with molten polyamide in open-air feed ports can generate crosslinked specks. Bynel 41E871 should be stored in unopened packaging below 50°C and processed with adequate nitrogen blanketing only when the line is stopped for more than 4 h. Published data for specific multilayer adhesion values remains limited because peel strength depends on adjacent layer formulation, die geometry, and cooling rate.