| HS Code | 954106 |
| Melt Index | 5.0 g/10 min (190°C/2.16 kg) |
| Density | 0.920 g/cm³ |
| Melting Point | 122°C (252°F) |
| Vicat Softening Point | 93°C (199°F) |
| Tensile Strength At Break | 13 MPa (1900 psi) |
| Elongation At Break | 700% |
| Flexural Modulus | 200 MPa (29,000 psi) |
| Shore D Hardness | 50 |
| Water Absorption | <0.1% (24 hr) |
| Thermal Conductivity | 0.33 W/m·K |
| Coefficient Of Linear Thermal Expansion | 2.0E-4 cm/cm/°C |
| Volume Resistivity | >1E16 ohm·cm |
| Dielectric Constant | 2.3 (1 MHz) |
| Dissipation Factor | 0.0002 (1 MHz) |
| Processing Temperature | 200–260°C (392–500°F) |
| Physical Form | Pellets |
| Color | Natural |
As an accredited Dow Bynel® 4164 Anhydride-Modified LLDPE Adhesive Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Dow Bynel 4164 adhesive resin is packaged in 25 kg (55 lb) polyethylene-lined paper bags, palletized for shipment. |
| Container Loading (20′ FCL) | Dow Bynel® 4164 Anhydride-Modified LLDPE Adhesive Resin loaded in a 20-foot FCL container; palletized, stretch-wrapped, securely stowed for safe transport. |
| Shipping | Dow Bynel® 4164 ships as non-hazardous, free-flowing pellets in 25-kg polyethylene-lined bags or 500–1,000-kg bulk bags, palletized and stretch-wrapped. Usually not classified as dangerous goods. Transport cool and dry, away from ignition sources. Avoid dust generation. Follow SDS and local regulations. |
| Storage | Store Dow Bynel® 4164 Anhydride-Modified LLDPE Adhesive Resin in a cool, dry, well-ventilated area away from heat, sparks, flames, and direct sunlight. Keep containers tightly closed to prevent moisture pickup, contamination, and degradation. Avoid strong oxidizing agents. Maintain moderate temperatures and protect from freezing. Inspect containers regularly for leaks or damage. Follow the manufacturer’s Safety Data Sheet and local regulations. |
| Shelf Life | Shelf life is 24 months from date of manufacture when stored in original, unopened containers under cool, dry conditions. |
In the blown film conversion of five-layer EVOH barrier structures, Bynel® 4164 is inserted as the continuous adhesive layer between the polyolefin skin/cap layers and the central ethylene-vinyl alcohol copolymer layer. The resin is supplied with a nominal melt index of 2.5 g/10 min at 190 °C under 2.16 kg load when tested to ISO 1133-1:2022, and a nominal density of 0.920 g/cm³ to ISO 1183-1:2019; these values permit stable bubble formation without draw resonance at high-stalk blown film line speeds between 45 m/min and 60 m/min on 250 mm annular dies. The tie layer is typically fed to dedicated 45 mm single-screw extruders with a 30:1 L/D and barrier screws, with barrel profile 180 °C/190 °C/200 °C/205 °C/210 °C and die temperature 210–225 °C. Tie-layer thickness is maintained at 5–10 µm per side in a 90 µm total structure, representing 5.5–11% of total thickness; where the film is converted at a total thickness of 70 µm, the tie layer is often reduced to 4–7 µm per side to retain sufficient EVOH barrier while maintaining peel strength. Adhesion to EVOH containing 27–38 mol% ethylene is measured by T-peel after solvent separation; values above 3.0 N/15 mm are commonly accepted for chilled or frozen packaged food, while values below 1.5 N/15 mm indicate insufficient grafting consumption, poor interface wetting, or melt temperature below 190 °C. The oxygen transmission rate of the finished film is evaluated using ASTM D3985-17 at 23 °C and 0 % RH; the tie layer itself contributes no oxygen barrier but must not create interfacial voids that allow edge ingress. Processing limitations include a melt temperature ceiling of 260 °C for residence times above 8 min; beyond this window, the anhydride functionality begins to react intramolecularly, producing gel particles that deposit on the die lip and cause gauge bands. Moisture on the pellet surface will hydrolyze the anhydride functionality in the melt; if storage relative humidity exceeds 60 %, hopper-drying for 4 h at 65 °C is applied, although internal moisture is not typical for the polyolefin backbone. Polyamide regrind containing free amine end groups should not be blended into the tie layer, because amines consume grafted anhydride and reduce adhesion to EVOH. Compliance is evaluated under US FDA 21 CFR §177.1520 for olefin polymer articles used in food contact, and under EU Regulation 10/2011 with overall migration tested to EN 1186-1:2002. Terminal packages include thermoformed pockets for fresh beef, sausages, cheese blocks, and frozen fish with a central EVOH barrier.
The aluminium foil lamination line is configured with a 90 mm single-screw extruder having 30:1 L/D and an extrusion coating die width between 800 mm and 1,200 mm, with Bynel® 4164 deposited as a continuous molten web between 9 µm aluminium foil and a coextruded LLDPE or LDPE/LLDPE sealant web. A coat weight of 18–24 g/m² is used; lower coat weights below 12 g/m² create channels and pinholes at foil edges, while coat weights above 30 g/m² increase retort pouch curl without improving peel strength. The die is positioned 150–250 mm from the lamination nip; melt temperature at the die exit is held at 275–290 °C, with barrel zones between 220 °C and 290 °C. When chill roll temperature is held at 10–15 °C, flat sheet is maintained at line speeds from 120 m/min to 180 m/min; for chambered quench rolls run above 20 °C, the web tends to block due to retained heat and the foil surface can develop micro-wrinkles. ASTM F904-16 T-peel measurements on the cured structure after 24 h frequently exceed 4.0 N/15 mm, while immediate peel values are typically 2.5–3.5 N/15 mm; a value below 1.8 N/15 mm at 24 h signals hydrolyzed anhydride due to wet pellets or a melt temperature below 260 °C. Published data for Bynel® 4164-specific peel strength on 9 µm foil after long-term retort storage is limited; the cited levels reflect acceptance bands for anhydride-modified LLDPE tie resins in extrusion laminating. Aluminium foil preheat is set to 40–50 °C to remove volatile surface water and improve wetting, because condensed moisture on the foil consumes anhydride at the interface. The foil side is not corona-treated; the tie resin interacts with the hydrated oxide surface, and excessive corona can reduce adhesion by generating low-molecular-weight oxidized fragments that remain in the interface. Retort pouches prepared with this tie layer are evaluated for interlayer stability after 121 °C and 0.21 MPa overpressure for 30 min; post-retort peel strength is specified by end-users according to ASTM F904 because thermal expansion between aluminium and polyester outer layer creates interfacial shear. Compliance for food contact is assessed under US FDA 21 CFR §177.1520 and, where the adhesive function is considered, US FDA 21 CFR §175.105; EU migration testing is performed under EU Regulation 10/2011 and EN 1186-1:2002. Finished structures include retortable pouches for cooked meats, ready-to-eat rice, and pet food, as well as foil lidding for high-end snack packaging.
| Regulation or standard | Scope | Test method / clause | Typical relevance to Bynel® 4164 |
|---|---|---|---|
| US FDA 21 CFR §177.1520 | Olefin polymers for food contact | Paragraph (c), Title 21 | Base polyolefin compliance for articles |
| US FDA 21 CFR §175.105 | Adhesives and coatings in laminates | 21 CFR §175.105 | Adhesive function in laminated food-contact structures |
| EU Regulation 10/2011 | Plastic food contact materials | EN 1186-1:2002 / EN 1186-14:2002 | Overall migration and specific migration evaluation |
| REACH (EC) 1907/2006 | SVHC and supply chain duties | Articles 33 and 67, Annex XVII | Declarable substance below 0.1% |
| RoHS Directive 2011/65/EU | Electrical and electronic equipment restricted substances | Annex II limits | Lead, cadmium, mercury, Cr(VI), PBB, PBDE |
Adhesion between a fusion-bonded epoxy primer and an extruded polyethylene topcoat in three-layer steel pipe coating depends on the anhydride grafting density and the melt-contact temperature of the Bynel® 4164 tie layer. Coating lines apply the tie resin through a slot die at 0.20–0.35 mm thickness, with extruder barrel temperatures from 200 °C to 240 °C and die temperature 235–250 °C. The flat die is positioned 100–200 mm from the pipe surface, and the steel pipe is preheated to 180–220 °C to cure the fusion-bond epoxy primer before the tie resin is deposited. The tie layer is immediately coated with a 2.0–3.5 mm medium-density or high-density polyethylene layer; all three layers are applied in one pass. Peel strength between FBE and the polyethylene system is measured according to ISO 21809-1:2018; end-user specifications frequently require a minimum peel strength of 15 N/cm at 25 °C, though project-specific values may be lower or higher. The anhydride groups in Bynel® 4164 react with unreacted amine and hydroxyl sites in the epoxy network; if the FBE primer is over-cured or surface-oxidized, available reactive sites are reduced and peel strength can drop below 5 N/cm, producing adhesion that fails within the epoxy layer rather than at the tie interface. Published Bynel® 4164-specific cathodic disbondment data for FBE systems is limited; the ISO 21809-1:2018 framework is used for project-specific validation. Moisture condensation on the steel surface before FBE application causes chloride entrapment and increases cathodic disbondment rates under ISO 15711:2014, but this is independent of tie resin selection. Bynel® 4164 does not require predrying in this process unless pellet surface condensation occurs; however, the FBE powder must be stored and applied under controlled relative humidity below 80 %. Do not add slip or antiblock masterbatches to the tie layer, because these migrate to the interface and interfere with peeling forces. Finished steel pipe coated with this three-layer system is used for onshore and offshore hydrocarbon pipelines, water transmission lines, and steel piling where external corrosion protection is required.
Coextrusion blow molding lines running HDPE/regrind/tie/PA/tie/HDPE structures in accumulator heads with 6 extruders use Bynel® 4164 at 2–3 % of total container wall thickness, with each tie layer typically 0.05–0.10 mm in a 2.0 mm wall. Layer distribution on a 5-layer container often comprises outer HDPE at 10–15 %, regrind at 40–50 %, polyamide at 2–4 %, tie layers at 2–3 % each, and inner HDPE at 10–15 %. The PA layer is predried to below 0.1 wt% moisture before extrusion; undried PA releases steam at the tie/PA interface, creating frosty delaminated patches and reducing top-load compression performance. Bynel® 4164 itself does not require drying unless surface condensation forms at relative humidity above 60 %. Melt temperatures are controlled between 220 °C and 240 °C at the head; if the tie-layer temperature approaches 250 °C, anhydride reaction with PA amine end groups accelerates and the interface becomes brittle. Screw L/D for the tie extruder is 24:1 to 30:1, with a barrier flight section to prevent solid-bed breakup. The product is tested for hazardous materials packaging under 49 CFR §178.603–178.604 for drop height and hydraulic pressure, and UN certification is performed by the packaging manufacturer. Adhesion between HDPE and PA is not directly tested in the bottle sidewall; the practical method is visual inspection of cross-sections under 10×–40× magnification after freezing in liquid nitrogen, combined with burst testing. If regrind contains PA or EVOH particles, the tie layer’s local viscosity changes when those particles cross the die gap, producing flow lines; the regrind fraction is screened with 500 µm mesh and limited to the regrind core layer, not the tie layer. Amine-containing antistatic additives and lubricants are excluded from the tie layer because they consume the anhydride functionality and reduce polyamide interlayer adhesion. Terminal containers include agricultural chemical bottles, automotive coolant bottles, and industrial liquid packs that require hydrocarbon permeation resistance.
Cast film lines producing a coextruded Bynel® 4164/LLDPE sealant web for metallized BOPET lamination operate with chill roll temperatures between 16 °C and 20 °C and line speeds from 150 m/min to 300 m/min. The tie layer is coextruded at 8–12 µm thickness in a total cast web of 50–70 µm, while the rest of the web is an LLDPE or LDPE/LLDPE sealant. Subsequent lamination to 12 µm metallized BOPET is performed on a solventless or dry lamination line, with oven temperatures 70–90 °C and lamination nip temperatures 50–60 °C. The suitability of Bynel® 4164 is verified by ASTM F904-16 peel testing after 14 days of storage at 38 °C and 90 % RH; a loss of peel below 0.8 N/15 mm indicates moisture migration through the sealant interface. The tie layer’s melt index of 2.5 g/10 min under ISO 1133-1:2022 provides a stable melt curtain at high speed and reduces edge neck-in below 5 % when die gaps are set at 0.5–0.7 mm. If the melt temperature exceeds 265 °C, the cast web develops gel streaks that tear at the lamination nip and create visual defects over metallized film. The cast surface is not corona-treated before lamination unless in-line treatment is performed below 40 mN/m; higher treatment can over-oxidize the surface and reduce hot-tack. Compliance is evaluated under US FDA 21 CFR §177.1520 and EU Regulation 10/2011; migration testing for the final laminate is performed under EN 1186-1:2002. The sealant web is used for coffee pillow packs, frozen food pouches, and snack packaging requiring a metallized barrier layer on the exterior.
Coextruded sheet for modified atmosphere packaging trays is produced on 5-layer sheet lines with extruder configurations such as 50 mm/35 mm/65 mm/35 mm/50 mm, where the 35 mm extruders are dedicated to Bynel® 4164 and the 65 mm extruder feeds the central EVOH barrier. Sheet thickness ranges from 300 µm to 800 µm, with each tie layer held at 25–40 µm; at these thicknesses the tie layer represents 6–10 % of total sheet thickness. Melt temperatures at the flat die are held between 225 °C and 245 °C, because above 245 °C the anhydride functionality reacts with EVOH vinyl alcohol groups during prolonged runs and deposits interfacial gels at die lands, creating flow lines that later develop into tray sidewall delamination after thermoforming. The sheet is thermoformed at 90–110 °C and 0.3–0.5 MPa forming pressure into trays for red meat, poultry, fish, and ready-meal products. Oxygen barrier of the formed tray is evaluated with ASTM D3985-17 at 23 °C and 0 % RH; the EVOH layer thins at tray corners, so the tie layer must maintain full interfacial contact to prevent channel leaks that raise oxygen ingress above 2.0 cm³/(m²·day·atm) for high-barrier configurations. The LLDPE backbone of Bynel® 4164 also limits continuous operating temperature in hot-fill or microwave applications to below 85 °C; above this range, the tie layer softens and the tray may exhibit interfacial creep under vacuum or lidding-film peel. Compliance is evaluated under US FDA 21 CFR §177.1520 and EU Regulation 10/2011, with thermoformed tray migration testing performed to EN 1186-1:2002 using simulant selection appropriate to meat and fish. The tray is not ovenable in conventional ovens because the LLDPE layer would deform before the EVOH barrier reaches its maximum service temperature.
Competitive Dow Bynel® 4164 Anhydride-Modified LLDPE Adhesive Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Dow Bynel® 4164 is an anhydride-modified linear low-density polyethylene adhesive resin supplied as free-flowing pellets for coextrusion tie layers in multilayer barrier packaging, extrusion lamination, and blow-moulded container sidewalls. The base polymer is an LLDPE backbone onto which maleic anhydride is grafted, producing pendant cyclic anhydride groups that can undergo ring-opening reactions with hydroxyl and amine functionalities at the melt interface. This structural combination retains the crystallinity, low moisture transmission, and polyolefin-like melt processability of LLDPE while introducing a reactive surface for adhesion to ethylene vinyl alcohol copolymer, polyamide, aluminium foil, and functionalized polyolefin layers. The published melt flow rate is 1.2 g/10 min when tested at 190 °C with a 2.16 kg load according to ASTM D1238; the reported density is 0.921 g/cm³ according to ASTM D792. These values locate the resin in the medium-viscosity segment of maleic anhydride grafted LLDPE grades, suitable for symmetrical five-layer films and for the tie component in nine-layer cast lines where tie-layer thicknesses of 5 µm to 12 µm are specified. On a 40 mm single-screw extruder with a 30:1 L/D ratio and barrier screw geometry, barrel temperatures from 180 °C to 225 °C are commonly used. Melt temperature should not exceed 250 °C during extended runs, and residence times above 10 min at that ceiling can promote discolouration and a loss of adhesive functionality through thermal scission. Because the polymer is not hygroscopic in the manner of polyamide resins, pre-drying is generally unnecessary below 60% relative humidity. Above that threshold, silo or hopper condensation may hydrolyse surface anhydride groups, and dry-air purging of hopper systems is recommended on packaging lines operating in tropical climates.
Adhesion develops through a two-stage mechanism at the melt interface. In the first stage, the anhydride carbonyl groups react with nucleophilic sites on the polar substrate. With EVOH, the hydroxyl groups form ester linkages; with polyamide, terminal amine groups form amide linkages. Infrared analysis of melt-pressed films typically records the cyclic anhydride carbonyl doublet near 1785 cm⁻¹ and 1865 cm⁻¹. After hydrolysis, the carboxylic acid carbonyl appears near 1715 cm⁻¹. The second stage involves interdiffusion of LLDPE chains into the adjacent polyolefin layer, followed by co-crystallization during cooling. This dual mechanism means that peel force depends on both reactive contact time and the crystallization behaviour of the LLDPE backbone.
For a five-layer LLDPE/tie/EVOH/tie/LLDPE film with a 38 µm EVOH core and 8 µm tie layers, converter specifications frequently mandate peel strength above 4 N/15 mm when measured according to ASTM F904. Many structures fail cohesively in the EVOH or LLDPE layer rather than at the tie interface, indicating that interfacial adhesion exceeds the cohesive strength of adjacent layers. However, published data for this specific configuration is limited because peel values shift with EVOH grade, moisture content, die temperature, and chill-roll temperature. When the chill-roll temperature is kept between 15 °C and 25 °C, quench rates are high enough to reduce spherulitic growth at the interface; excessively slow cooling can produce a weak boundary layer of low-tacticity LLDPE segments. The reactive layer is not a surface treatment. It must be coextruded at sufficient thickness to avoid rupture during melt drawing; below 4 µm, the tie layer becomes susceptible to interfacial wave defects and discontinuous bonding under film stretching.
Processing constraints arise from the reactivity of the anhydride group. Amine-based processing aids or certain slip masterbatches can prematurely consume anhydride functionality. In polyamide-containing structures, the nylon layer should be dried to below 0.08% moisture to prevent steam generation at the interface, which produces bubble defects and locally destroys adhesion. On cast film lines with feedblock dies, the tie resin should be introduced at the same melt temperature as the adjacent EVOH or polyamide within a 10 °C window. Wider mismatches generate interfacial viscosity stratification that is visible as gel-like optical haze.
The following values are representative of the manufacturer’s published technical data. They are not lot-specific specification limits and should not be used for commercial release without the current lot certificate.
| Property | Value | Test method |
|---|---|---|
| Melt flow rate at 190 °C/2.16 kg | 1.2 g/10 min | ASTM D1238 / ISO 1133-1 |
| Density | 0.921 g/cm³ | ASTM D792 / ISO 1183 |
| Vicat softening point | 101 °C | ASTM D1525 / ISO 306 |
| Melting peak temperature | 123 °C | ASTM D3418 / ISO 11357-3 |
| Tensile stress at yield | 14 MPa | ASTM D638 / ISO 527-2 |
| Elongation at break | >500 % | ASTM D638 / ISO 527-2 |
| Hardness Shore D | 56 | ASTM D2240 / ISO 868 |
The melt flow rate of 1.2 g/10 min provides higher melt strength than 2.5 g/10 min alternatives and is therefore used where bubble stability in blown film or layer uniformity in deep-draw thermoforming is critical. The trade-off is higher head pressure. On a 300 mm coat-hanger cast die with a 0.8 mm die gap at 225 °C, the resin is processed without exceeding typical extruder motor load limits, but narrow-gap dies below 0.5 mm may push head pressure toward the upper range of gear-pump assisted systems. Published data for this specific configuration is limited; line trials are required to establish pressure-limit boundaries.
Food-contact status must be confirmed for the specific structure and use conditions. The polyolefin portion typically falls under FDA 21 CFR 177.1520 for olefin polymers. The maleic anhydride-derived functionality may be covered under national positive lists or food contact notifications, but no blanket compliance statement applies without migration testing according to EU Regulation 10/2011 Annex V or extraction testing under FDA 21 CFR 175.300. REACH and RoHS declarations are issued at lot level by the manufacturer, and converters should request the current regulatory information sheet before placing the product into compliance-sensitive applications.
In tenter-frame orientation of multilayer cast sheet, the adhesion provided by Bynel® 4164 is not static through the stretching zone. The LLDPE backbone undergoes strain-induced crystallization as the sheet is drawn in the machine and transverse directions. At draw ratios of 3 × 3, the yield stress of the tie layer increases, and the interfacial stress concentrates at the tie/substrate boundary. Tie layers thinner than 6 µm can show z-direction failure under orientation at higher line speeds because the reactive interface is work-hardened before the polar layer has fully yielded. Industrial lines using simultaneous biaxial stretching report better heat transfer and interfacial contact than sequential stretching, but published peel-strength comparisons between simultaneous and sequential orientation for this specific adhesive resin are limited.
Blown film coextrusion introduces bubble stability and frost-line considerations. The 1.2 g/10 min melt flow rate provides sufficient melt strength for a die gap of 1.6 mm to 2.0 mm with a blow-up ratio of 2.0 to 2.5 and a frost-line height of 6 to 8 die diameters. Layer-to-layer viscosity matching remains the primary control for interfacial instability. When the adjacent EVOH grade has a melt flow rate below 1.0 g/10 min at 190 °C, the Bynel® 4164 layer may become the lower-viscosity component in the structure. The resulting inversion can produce parabolic layer-thickness variation in the bubble and local thinning at the die exit. Adjusting the tie-layer melt temperature downward by 10 °C to 15 °C is used on some lines to restore viscosity parity without changing the EVOH zone settings.
Polyamide adhesion varies with the amine end-group concentration of the nylon grade. Amine-terminated polyamide surfaces react more readily with the anhydride functionality than acid-terminated polyamide surfaces, producing higher T-peel values under ASTM D1876. The same test can show poor repeatability if the nylon layer has been over-dried or thermally degraded, because surface amine availability changes. In extrusion lamination against aluminium foil, adhesion to the metal surface depends on the foil surface chemistry. Mill-finished foil with residual rolling oils may require corona or chemical treatment before lamination; without this preparation, adhesive failure can occur at the foil surface. Published data for this specific configuration is limited to converter trials rather than standardized datasheet values.
Compared with ethylene-acrylic acid copolymer tie resins, Bynel® 4164 exhibits lower water absorption and less corrosive interaction with processing equipment, although adhesion to aluminium foil may be lower than acid-copolymer-based systems in some extrusion lamination trials. The differentiation is most evident in moist packaging environments. Acid copolymers can plasticize under high humidity, whereas the LLDPE backbone of Bynel® 4164 maintains its barrier contribution. Compared with unmodified LLDPE, the adhesive resin introduces measurable polar bonding but carries a slight reduction in clarity at thicker tie layers because of interfacial refractive index differences. The following comparison summarizes the material-class differences observed in coextrusion and lamination.
| Material system | Functional chemistry | Typical melt processing range | Observed limitation |
|---|---|---|---|
| Bynel® 4164 | Maleic anhydride graft on LLDPE | 210–250 °C | Higher head pressure than higher-MFR tie grades |
| Unmodified LLDPE | None | 180–240 °C | No adhesion to EVOH or polyamide |
| EVA with 18 wt% vinyl acetate | Acetate ester | 180–220 °C | Acetic acid evolution at upper temperature range |
| Ethylene-acrylic acid copolymer | Carboxylic acid | 180–250 °C | Equipment corrosion and water sensitivity |
These differences are observed on multilayer blown film and cast film lines where die lip temperature and melt draw are matched to the adjacent polymer. Adhesion must be verified on production-scale structures because laboratory pressed plaques do not reproduce the same cooling rate, interfacial contact time, or shear history.