| HS Code | 883408 |
| Product Name | CIPLAS LLF2019F |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Grade Type | Film Grade |
| Comonomer | Butene-1 |
| Catalyst Type | Ziegler-Natta |
| Form | Pellets |
| Density | 0.919 g/cm3 |
| Melt Flow Rate 190 C 2 16 Kg | 2.0 g/10 min |
| Melt Flow Ratio I21 I2 | 25-30 |
| Melting Point | 122 °C |
| Crystallization Temperature | 105 °C |
| Vicat Softening Point | 92 °C |
| Tensile Strength At Yield | 10 MPa |
| Tensile Strength At Break | 22 MPa |
| Elongation At Break | 700 % |
| Flexural Modulus | 240 MPa |
| Dart Impact Strength | 110 g |
| Elmendorf Tear Strength Md Td | 150/300 g |
| Haze | 12 % |
| Gloss 45 | 50 % |
| Blocking | 80 g |
| Coefficient Of Friction | 0.2 |
| Bulk Density | 0.57 g/cm3 |
| Molecular Weight Distribution | Narrow |
| Additives | Antioxidant, slip, anti-block |
As an accredited CIPLAS LLF2019F Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | CIPLAS LLF2019F Linear Low Density Polyethylene is supplied in 25 kg polyethylene-lined woven sacks, palletized for industrial handling and storage. |
| Container Loading (20′ FCL) | CIPLAS LLF2019F Linear Low Density Polyethylene is loaded into a 20′ FCL, typically palletized 25 kg bags, approximately 20 metric tons. |
| Shipping | CIPLAS LLF2019F Linear Low Density Polyethylene is typically shipped as non-hazardous thermoplastic pellets in 25 kg PE-lined bags, bulk bags, or bulk trucks/railcars. Keep dry, store below 50°C, away from ignition sources, and protect from UV. Transport per applicable regulations; no special hazardous shipping class. |
| Storage | Store in a cool, dry, well-ventilated area away from heat, sparks, open flames, and direct sunlight. Keep containers sealed and palletized off the floor to prevent moisture pickup and contamination. Avoid contact with strong oxidizers. Maintain stable ambient temperatures, avoid excessive stacking, and follow local regulations and supplier recommendations. Use original or compatible labeled containers and protect from physical damage. |
| Shelf Life | Shelf life: typically 24 months when stored unopened in a cool, dry, ventilated area away from direct sunlight. |
For monolayer blown film conversion of CIPLAS LLF2019F on a 65 mm single-screw extruder equipped with a L/D 30:1 barrier screw and Maddock mixing element, the die gap is set at 1.8–2.2 mm rather than the narrower 1.0–1.2 mm gap used for LDPE-dominant formulations. The certificate of analysis normally documents a melt flow rate of 1.9 g/10 min at 190 °C/2.16 kg per ISO 1133-1:2022 and a density of 0.920 g/cm³ per ISO 1183-1:2019. Melt temperature at the feed throat should be maintained at 190–230 °C, with the die zone held at 205–220 °C, because this linear resin does not develop the long-chain branching required for stable bubble expansion at temperatures above 230 °C. A dual-lip air ring with internal bubble cooling is preferred for gauge uniformity when the blow-up ratio is maintained between 2.0:1 and 3.0:1; the frost line height is normally controlled between 600 mm and 900 mm above the die face to prevent the high-stalk bubble from entering a resonant flutter mode. Antiblock masterbatch is introduced at 5,000–10,000 ppm and slip additive at 500–1,000 ppm to support film separation and unwind behaviour in downstream bag-making lines. Tensile properties are evaluated according to ISO 527-3:2018, Elmendorf tear resistance according to ISO 6383-2:1983, and dart impact resistance according to ASTM D1709-16a. The material is used for general-purpose industrial liners, garment bags, and protective overwrap where high clarity is not the primary requirement. In high-humidity coastal storage at relative humidity above 60%, a desiccant pre-dryer set at 70 °C for 2 h is advisable before extrusion because surface moisture on pelletised feed can produce porosity in the film web even though the polyolefin matrix itself has negligible water absorption. No processing aid is required below shear rates of 500 s⁻¹, but melt pressure upstream of the screen pack should be logged continuously; an increase of more than 30% during an 8 h shift indicates screen pack occlusion and demands a filter basket change.
Bubble instability in linear low density polyethylene is dominated by the absence of strain-hardening extensional flow, which is a direct consequence of the molecular architecture of LLF2019F and similar butene-comonomer linear grades. When the blow-up ratio exceeds 3.0:1 on a high-stalk configuration with frost line height below 600 mm, the film bubble enters a periodic diameter oscillation that cannot be corrected by air volume changes alone. In this regime the orienting stress in the molten web is insufficient to resist ambient air turbulence, because the extensional viscosity fails to increase rapidly with strain rate in the way observed in LDPE-rich blends containing long-chain branching. Operators should therefore restrict blow-up ratio to 2.2:1–2.8:1 for film thicknesses below 40 µm, unless a high melt strength LDPE is added at 10–20 wt%. The addition of LDPE also broadens the bubble stability window and permits a shorter frost line, but it increases haze and reduces tensile strength in the machine direction. A second corrective measure is the use of a lower melt temperature towards 195–210 °C, which raises melt viscosity at the die and dampens oscillation. On lines equipped with internal bubble cooling, the IBC stack should be placed to stabilise the upper neck of the bubble before the frost line, and the external air ring should be adjusted to deliver a descending air profile that prevents the melt from fluttering at the die lip. Thickness scanning must be performed with an online capacitance or fast-magnetic gauge sensor, because the gauge variation at 3.0:1 blow-up ratio above the critical frost line distance can exceed ±8% on a 50 µm target. The failure mode for such film appears in bag converting as wandering seal position and splice-induced breaks during high-speed wicket punching. For end uses such as collation film, where consistent roll hardness is the acceptance criterion, the process window is deliberately narrowed to a frost line height of 700–850 mm and a blow-up ratio of 2.4:1–2.7:1. The rheological test for lot-to-lot control is not a simple melt flow ratio but the shear viscosity at 100 s⁻¹ obtained by capillary rheometry on a sample predried for 1 h at 60 °C, with drift limits referenced to the qualified production lot. The same test is used to qualify incoming railcar batches before extrusion, because a shift greater than 5% in that viscosity can move the stable blow-up ratio edge by more than 0.2:1, which is large enough to trigger extrusion rejects on thin-gauge lines. This application segment therefore represents a deep process-control interaction in which resin rheology, die temperature uniformity, frost line positioning, and air ring pressure must be treated as a single coupled parameter set.
In three-layer coex lamination films, CIPLAS LLF2019F is assigned to the sealant layer at layer ratios between 20% and 30%, with the core and skin layers built from HDPE, metallocene LLDPE, or polypropylene depending on the final laminate. The seal initiation temperature is governed by the broad melting region of the linear low density polyethylene, which is measured by differential scanning calorimetry according to ISO 11357-3:2018. When the lot certificate records a peak melting temperature between 121 °C and 125 °C, the observed heat seal initiation is generally 15–25 °C below that peak under a 0.5 s dwell and 0.28 MPa sealing pressure on a flat-platen laboratory sealer. Hot tack is measured according to ASTM F1921-18 with a cooling time of 50 ms and a peel speed of 200 mm/min, and the usable hot tack window for this sealant resin falls within the seal bar temperature band of 105–125 °C. Below 105 °C, the interface does not develop enough molten interdiffusion, while above 125 °C the sealant layer begins to squeeze towards the film edge and creates a weak peripheral seal during vertical form-fill-seal operation. Slip additive at 500–700 ppm and antiblock at 3,000–5,000 ppm are the standard surface-modification package, but the slip level must be verified after printing and lamination because surface bloom can reduce seal strength by more than 15% if uncontrolled over 30 days of roll storage. The extrusion process for the sealant layer uses a 45 mm satellite extruder with L/D 28:1, and the melt pipe is maintained below 220 °C to prevent gel formation at stagnant flow boundaries. Film seal strength is reported as the peak force per 15 mm width according to ASTM F88/F88M-21, and the lamination converter applies an acceptance minimum of 8 N/15 mm for dry-food pouches after conversion. The end products include dry food pouches, sachet laminates, and overwrap for soap and personal care cartons. In direct contact applications, the compound must satisfy the regulatory matrix below, and the converter must retain batch-specific certificates of analysis for the base resin, masterbatches, and the final printed structure, because the liability chain under EU food contact law extends to the packaging converter.
| Regulation or Standard | Specific Requirement | Application Condition |
|---|---|---|
| FDA 21 CFR 177.1520 | Olefin polymers intended for food contact | End-use temperature conditions A through H must be matched to the packaged food type |
| EU 10/2011 | Plastic materials and articles for food contact | Overall migration limit 10 mg/dm²; specific migration limits for monomers such as ethylene and butene must not exceed set values in Annex II |
| REACH 1907/2006 | SVHC candidate list compliance | No SVHC intentionally added; article-level communication duties under Article 33 apply if candidate list substances exceed 0.1% by weight |
| RoHS 2011/65/EU | Heavy metal and restricted substance limits | Pb 1,000 ppm, Cd 100 ppm, Hg 1,000 ppm, Cr VI 1,000 ppm, PBB and PBDE 1,000 ppm each |
On a cast film line with a 1,500 mm wide coat-hanger die, LLF2019F is processed at melt temperatures of 240–260 °C and a die gap of 0.5–0.8 mm, with the air gap held between 10 mm and 20 mm to limit neck-in before the chill roll. The chill roll surface temperature is maintained at 20–30 °C, because lower surface temperatures increase chill roll adhesion and cause transverse web wrinkles, while higher surface temperatures reduce film gloss and slow the crystallisation front. Edge trim from the cast line is reintroduced into the extruder feed at 15–30 wt%, but only after the trim is ground to an average pellet size below 5 mm and blended in a weigh-hopper to avoid screw bridging. This closed-loop recycle is a major process bottleneck because polyisobutylene tackifier added for pallet wrap at 1–3 wt% concentrates in the recycled fraction and promotes die lip deposition after 8–12 h of continuous operation. The cling agent is characterised by low migration resistance in the amorphous LLDPE matrix, and the resulting plate-out on the chill roll and die lip is removed by operator intervention during scheduled line stops. Cling performance is measured according to ASTM D5458-95(2020) for peel cling and ASTM D5748-19 for puncture resistance, with the film specified at 17–25 µm thickness for high-performance machine wrap. Stretch force and retained load are evaluated on a constant-rate-of-extension tester at 200%/min extension, and the target retained load after 100% stretch is above 60% of the initial force. The product is shipped in roll diameters of 200–500 mm, and the immediate packaging must be a polyethylene shroud that does not absorb the tackifier from the film surface. A storage temperature above 35 °C is avoided because cling additives can migrate to the film core within 30 days, causing unacceptable unwinding force decline on automatic pallet wrapping machines. This cast stretch film segment uses LLF2019F only in monolayer or skewed-layer structures where a high-molecular-weight tackifier is incorporated; in five-layer high elongation stretch lines, the grade is typically blended with a lower-density metallocene LLDPE to raise strain hardening without losing cling uniformity.
Agricultural silage cover and ensiling film manufactured from LLF2019F is specified at thicknesses between 100 µm and 180 µm and must retain mechanical integrity after extended outdoor exposure. The film is produced on a three-layer blown line with a 400 mm spiral mandrel die, a die gap of 2.0 mm, and a blow-up ratio of 2.5:1, because the black masterbatch used for opacity alters melt viscosity and requires a wider die gap to prevent die lip shear at the outer mandrel ports. Carbon black masterbatch is added at 6–8 wt% of a 40% black concentrate to achieve final carbon black content of 2.4–3.2 wt%, with primary particle size specified below 50 nm and dispersion quality controlled by pressure rise across the screen pack. A hindered amine light stabilizer system is introduced at 0.10–0.25 wt% active across the three layers, with the highest concentration placed in the outer layer that faces solar radiation. Accelerated weathering is conducted according to ISO 4892-2:2013 using xenon-arc exposure with a daylight filter, black standard temperature of 65 °C, and a 1,020 min dry / 180 min wet cycle. The acceptance criterion for silage cover is at least 50% retained elongation at break after 2,000 h of exposure, although published data for this specific film configuration is limited and field trials under high-UV mountain conditions are required before multi-year warranties. The tensile properties after dark storage and after accelerated weathering are measured according to ISO 527-3:2018, and tear resistance is measured according to ISO 6383-2:1983. Oxygen transmission rate at 23 °C and 0% relative humidity for the 150 µm film is evaluated by ASTM D3985-17, with a typical reported band for this application around 1,500–2,800 cm³/(m²·day·atm), and it is used to assess the anaerobic ensiling environment rather than as a high-barrier specification. European agricultural film compliance is verified against EN 13206:2017 for thermoplastic covering films used in agriculture and horticulture, including thickness classification and solar transmission limits for black film. The process limitation is that the carbon black-filled melt requires a higher extruder load, and the outer layer melt temperature is held at 215–225 °C to avoid thermal decomposition of the HALS package. The film is converted into clamp silage covers, fermentation sealing films, and temporary bunker covers, and the edge folds are welded at 150 °C with an overlap of 40 mm to create gas-tight joins that prevent oxygen ingress after compaction. A shallow-zone practice within this segment is the use of seam welding, which requires only a pedal-operated wedge welder and does not require further formulation adjustment.
Heavy-duty shipping sacks and valve bags in the 80–150 µm thickness range are produced by blending LLF2019F with tubular LDPE at 10–20 wt%, because the LDPE fraction supplies the bubble stability and melt curtain stiffness required for high-output lines running above 120 kg/h. The blown film line for this segment is configured with a 75 mm main extruder and a 350 mm die, the die gap is set at 2.0–2.4 mm, and the blow-up ratio is limited to 2.0:1–2.6:1 to provide the transverse direction tear resistance expected in filled sack drops. Dart impact strength is measured according to ASTM D1709-16a using Method A, tensile properties according to ISO 527-3:2018, and tear strength according to ISO 6383-2:1983. A smooth slip package is required for high-speed form-fill-seal conversion, with erucamide at 600–900 ppm and synthetic silica at 2,000–3,000 ppm, because the sack surfaces must not block during winding after corona treatment on the outer print skin. The corona treatment intensity is set to 38–42 dyn/cm for solvent-based flexographic inks, and the treated film is converted within 24 h to prevent surface decay below the ink adhesion threshold of 36 dyn/cm. The main process failure in this segment is drop-test failure at the sack seal corner, which typically originates from gauge variation above ±10% at the gusset fold, and that variation is controlled by an online thickness scanner coupled to the die bolt heater system. The LDPE dilution is adjusted within the 10–20 wt% window based on the ambient temperature of the production hall; at air temperatures below 20 °C the lower LDPE level is favoured to avoid excessive stiffness, while above 30 °C the upper level is used to maintain bubble equilibrium. End products include fertiliser sacks, resin granule bags, and industrial parts bags with welded valve inserts, and the converting line speed is limited by the heat seal window of the LLDPE-dominant sealant surface rather than by the printing station.
Competitive CIPLAS LLF2019F Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
CIPLAS LLF2019F Linear Low Density Polyethylene is a film-grade ethylene/α-olefin copolymer manufactured under the CIPLAS brand by Brahmaputra Cracker and Polymer Limited. The grade nomenclature follows a supplier convention in which the numerical field is read as a nominal melt mass-flow rate of 1.9 g/10 min at 190°C/2.16 kg per ISO 1133-1:2022, and the terminal F marks film extrusion as the intended conversion route. The base polyethylene polymer is described by CAS 9002-88-4. The resin belongs to the linear low-density polyethylene class: the backbone is linear and contains short-chain branches introduced through α-olefin comonomer insertion, which lowers crystallinity relative to high-density polyethylene while retaining higher tensile and puncture resistance than branched low-density polyethylene at equivalent density. Because public lot-specific certificates for this exact grade are not consistently available in third-party repositories, the numerical envelope reported in the following sections is class-representative for film-grade LLDPE in the 0.918–0.922 g/cm³ density band and should be checked against the certificate of analysis for each production lot before setting machine parameters.
In blown film conversion, adapter and die temperatures are normally maintained between 180°C and 210°C. At melt temperatures above 230°C, oxidative chain scission and gel formation become increasingly probable under atmospheric conditions; at temperatures below 170°C, the high melt viscosity raises extruder pressure and can produce rough film surface. A flat-to-slightly-reverse thermal profile is commonly used: feed zone 160–170°C, barrel zones 170–190°C, adapter 190–200°C, and die 190–210°C.
A standard blown film line with a single-screw extruder of 25:1–30:1 L/D, a barrier feed section, and a Maddock-style distributive mixer is suitable for this grade. Annular die gaps of 1.8–2.4 mm are used in practice. Narrower gaps reduce melt residence time but increase shear rate and die build-up risk. A blow-up ratio of 2.0:1–3.0:1 is standard for heavy-duty film. Frost line height is often maintained at 6–8 die diameters to preserve dart impact; a higher frost line increases machine-direction orientation but may decrease transverse tear resistance.
Because the linear backbone produces less shear thinning than branched low-density polyethylene, motor load and die pressure are higher at the same melt index. Capillary rheometry per ISO 11443 on film-grade LLDPE of this melt flow index class shows an apparent viscosity of approximately 800–1,200 Pa·s at 190°C and 100 s-1, with a shear-thinning index between 100 s-1 and 1,000 s-1 of 0.55–0.65. This relatively low shear thinning explains the pressure sensitivity to die-gap reductions: reducing the die gap from 2.4 mm to 1.8 mm can increase die pressure by 15–25% on the same screw speed. Melt pressure before the screen pack on a 45 mm extruder is typically 250–350 bar during stable operation; the screw manufacturer's maximum thrust bearing limit should not be exceeded.
The bubble cooling rate is often the primary throughput constraint rather than screw recovery. A single-orifice air ring with air temperature 15–25°C and air velocity 8–15 m/s is sufficient for moderate output. When line speed is raised, the frost line height rises and film blocking risk increases unless the collapsing frame and idler rolls are maintained below 40°C. Internal bubble cooling is required on high-output lines above approximately 3.5 kg/h/cm of die circumference.
Downgauging trials on heavy-duty sacks, industrial liners, and lamination film are evaluated against minimum values for tensile stress, elongation, dart impact, and tear propagation. The class-representative values in Table 1 are reported for 25 µm blown film produced with a blow-up ratio near 2.5:1; directional values are machine direction and transverse direction.
| Property | Standard method | Typical class envelope | Relevance to conversion |
|---|---|---|---|
| Melt mass-flow rate | ISO 1133-1:2022 | 1.8–2.0 g/10 min at 190°C/2.16 kg | Controls extruder head pressure and throughput |
| Density | ASTM D1505 | 0.919–0.921 g/cm³ | Sets film stiffness, dart impact, and barrier balance |
| Tensile stress at yield | ISO 527-3 | 10–13 MPa MD / 9–12 MPa TS | Influences film handling and load resistance |
| Tensile stress at break | ISO 527-3 | 30–40 MPa MD / 26–35 MPa TD | Determines load-bearing capacity in sacks |
| Elongation at break | ISO 527-3 | 700–900% MD / 750–950% TD | Indicates film toughness during stretching |
| Dart impact, Method A | ASTM D1709 | 90–150 g | Key criterion for puncture resistance |
| Elmendorf tear | ASTM D1922 | 100–160 g MD / 120–180 g TD | Measures tear propagation resistance |
| Haze | ASTM D1003 | 8–14% | Controls optical clarity in packaging |
| Vicat softening temperature | ASTM D1525 | 88–95°C | Indicates onset of thermal softening |
The film property balance is controllable by modulation of blow-up ratio, frost line height, and die-gap residence time. Higher blow-up ratio shifts tensile balance toward the transverse direction and reduces machine-direction tear, while low frost-line cooling tends to improve dart impact but may increase haze if crystalline superstructures become coarse. In a standard three-zone collapsing frame, the film is edge-trimmed at the slitting station; trim scrap can be reintroduced in-line at up to 20 wt% unless optical haze is critical.
At 25 µm, LLDPE films in this density band exhibit water vapour transmission rates in the range of 18–25 g/m²·day at 38°C and 90% RH per ASTM F1249. Oxygen transmission rates are commonly 3,500–5,000 cm³/m²·day·bar at 23°C and 0% RH per ASTM D3985. These values are not intended as specifications but are useful for packaging engineers calculating shelf-life requirements.
On high-speed vertical form-fill-seal equipment, heat seal initiation for LLDPE film is generally 85–95°C, and the seal strength plateau is reached at 110–130°C with dwell 0.5–1.0 s and seal pressure 1–3 bar. The broad seal plateau permits line speeds above 40 cycles/min when the sealing jaw is maintained at 110–120°C.
Replacement of low-density polyethylene with CIPLAS LLF2019F in heavy-duty sacks, agricultural films, and industrial liners usually raises the load-bearing capacity at equal film gauge. The linear backbone and higher tensile stress at break permit downgauging of the film structure by 10–20% in many blown-film applications where dart impact governs. However, substitution is not direct on high-drawdown extrusion-coating lines because the melt lacks the long-chain branching of autoclave low-density polyethylene, resulting in lower melt strength and higher neck-in.
For extrusion-coating and high-drawdown processes, blending CIPLAS LLF2019F with low-density polyethylene at 20–40 wt% is commonly necessary to improve drawdown and reduce neck-in. In blown film, addition of low-density polyethylene at 10–30 wt% improves bubble stability and optics but reduces dart impact somewhat. The exact blend ratio should be determined on the target line because the influence of the blending partner depends on its melt index and long-chain branching density.
Compared with conventional butene-copolymer LLDPE of the same density and melt index class, CIPLAS LLF2019F occupies a similar property envelope; differentiation is often lot-dependent and line-dependent rather than architectural. Film property comparisons should use ASTM D1709 dart impact, ASTM D1922 Elmendorf tear, and ISO 527-3 tensile data generated on the same blown film line. Published data for this specific configuration is limited, and no direct grade-versus-grade ranking should be inferred without paired film samples.
Metallocene-catalysed LLDPE grades of equivalent density generally show better dart impact and lower seal initiation, but they commonly generate higher extruder head pressure and may require lower screw speeds or wider die gaps. CIPLAS LLF2019F, as a conventional linear-low polyethylene architecture, offers a broader processing window and is less sensitive to shear-induced melt fracture at standard die gaps; film clarity, however, is typically lower than that of metallocene film because of broader comonomer distribution.
Compared with high-density polyethylene at similar film thickness, LLDPE provides greater elongation, dart impact, and tear resistance but lower modulus and higher oxygen transmission. High-density polyethylene is preferred for stiffness-intensive packaging such as cereal liners, whereas LLDPE is preferred in heavy-duty sacks and liners where puncture resistance from angular granular contents is decisive.
Before commercial use in food-contact packaging, the converter must verify that the specific lot is formulated to meet FDA 21 CFR 177.1520 for olefin polymers and EU Regulation (EC) No 10/2011 with its migration limits under the intended food simulant. Under REACH Regulation (EC) No 1907/2006, polyethylene as a polymer is not subject to registration, but monomer and additive components must be registered and may be subject to authorisation or restriction. For fatty food simulants such as olive oil or 95% ethanol, migration testing is more severe than for aqueous simulants and should be conducted on the final film structure, not on the pellet.
The resin is not considered hygroscopic; however, storage in environments above 60% RH can allow surface condensation that creates localized melt voids if not removed. In such cases, pre-drying in a hopper dryer at 70°C for 2 h is sufficient before extrusion. Additive packages should avoid free halogenated species and strong mineral acids, which accelerate chain degradation at extrusion temperatures. Amine-based antistatic additives may promote surface bloom and affect seal strength unless explicitly recommended for the intended film structure.
Routine incoming inspection should include melt mass-flow rate per ISO 1133-1:2022, density per ASTM D1505, film dart impact per ASTM D1709, and visual gel count on a standard cast or blown film sample. Batch-to-batch variance in this product class is most commonly observed in gel count and odour, which are not fully captured by melt flow index and density alone. A fixed-condition film trial under target extruder temperatures is therefore required when changing supplier lots. The resin is not intended for injection moulding, blow moulding, or rotomoulding operations because the film-grade stabilizer package and melt rheology are not designed for long residence times in those tools.