| HS Code | 242285 |
| Density | 0.935 g/cm³ |
| Meltindex | 0.8 g/10 min |
| Meltingpoint | 124 °C |
| Vicatsofteningpoint | 110 °C |
| Tensilestrengthatyield | 2200 psi |
| Tensilestrengthatbreak | 5000 psi |
| Elongationatbreak | 600% |
| Flexuralmodulus | 80,000 psi |
| Dartdropimpact | 200 g |
| Elmendorftearmd | 250 g |
| Elmendorfteartd | 450 g |
| Haze | 12% |
| Gloss | 55% |
| Watervaportransmissionrate | 0.4 g/100 in²/24 h |
| Brittlenesstemperature | < -70 °C |
As an accredited Chevron Phillips mPact™ D353 m-MDPE Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Chevron Phillips mPact™ D353 m-MDPE LLDPE is supplied in 25 kg multiwall bags, palletized, or 1,000 kg bulk bags. |
| Container Loading (20′ FCL) | 20′ FCL loaded with palletized 25 kg bags of Chevron Phillips mPact™ D353 m-MDPE Linear Low Density Polyethylene, shrink-wrapped, secured. |
| Shipping | Chevron Phillips mPact™ D353 m-MDPE LLDPE resin is shipped as a non-hazardous solid in moisture-barrier bags, lined boxes, bulk trucks, or railcars. It is not regulated for DOT/IMDG/IATA transport. Store cool, dry, clean; avoid heat, sunlight, contamination. Follow SDS/local rules; use PPE and secure loads. Provide ventilation in storage areas. |
| Storage | Store Chevron Phillips mPact™ D353 m-MDPE Linear Low Density Polyethylene in a cool, dry, well-ventilated area away from direct sunlight, heat, and ignition sources. Keep containers sealed to prevent moisture, dust, and contamination. Place on pallets, off the floor, and use first-in/first-out rotation. Avoid prolonged outdoor exposure, excessive heat, and strong oxidizers. Follow the SDS and local regulations. |
| Shelf Life | No fixed shelf life if stored unopened in original packaging, cool, dry, ventilated conditions, away from sunlight, heat, moisture, and contaminants. |
mPact D353 m-MDPE is specified in geomembrane compounds where slow crack growth under sustained tensile load, rather than short-term yield strength, determines liner service life. The resin carries a nominal density of 0.933 g/cm³ per ASTM D1505 and a melt flow rate of 0.5 g/10 min at 190°C/2.16 kg per ASTM D1238. The lower crystallinity relative to HDPE reduces notch sensitivity at wrinkle stress concentrations and increases time to brittle failure in ASTM D5397 single-point notched constant tensile load testing at 50°C in 10% Igepal CO-630.
Compliance for this application is governed by project specifications that adapt GRI GM17 for LLDPE geomembranes and the test framework of GRI GM13 for HDPE liners, with MDPE-specific density and oxidative induction time limits inserted by the specifying engineer. Routine release testing includes ASTM D6693 tensile properties, ASTM D1004 tear resistance, ASTM D4833 puncture resistance, ASTM D5885 oxidative induction time, and ASTM D5397 stress crack resistance. A typical smooth geomembrane formulation contains 96.5–97.5 wt% mPact D353, 2.0–3.5 wt% carbon black masterbatch at 40% carbon black concentration, and 0.1–0.3 wt% antioxidant/process stabilizer masterbatch, yielding 2.0–2.5 wt% carbon black content. Carbon black dispersion is confirmed by ASTM D5596.
Production is performed on flat-die sheet extrusion lines with single-screw extruders having L/D ≥ 30:1, screen pack arrangement 100/120/120 mesh, and melt temperatures between 200°C and 230°C. The polished or textured three-roll stack is held at 60–90°C to control surface gloss and heat-set the sheet. Final liner thickness ranges from 1.0 mm to 2.5 mm for smooth profiles; textured profiles require embossing rolls or nitrogen gas injection. For blown-film geomembrane variants, the die gap is set at 1.5–2.5 mm and the blow-up ratio is maintained between 2.0:1 and 3.0:1. A critical processing boundary exists at 230°C: above this melt temperature metallocene polyethylene may generate odor-causing degradation products, while below 200°C melt pressure rises and carbon black dispersion deteriorates.
| Property | Standard | Geomembrane-specific purpose |
|---|---|---|
| Density | ASTM D1505-18 | Resin classification and carbon black correction |
| Melt flow rate | ASTM D1238-20 | 190°C/2.16 kg batch consistency |
| Tensile properties | ASTM D6693-18 | Break strength and elongation for seam design |
| Tear resistance | ASTM D1004-21 | Installation damage resistance |
| Puncture resistance | ASTM D4833-21 | Aggregate puncture during placement |
| Oxidative induction time | ASTM D5885-21 | Long-term oxidation stability of stabilizer package |
| SP-NCTL | ASTM D5397-20 | Stress crack resistance under sustained load |
Terminal products include smooth and textured geomembrane panels for landfill caps, secondary containment berms, canal liners, floating covers, and agricultural wastewater impoundments.
Rotational molding of mPact D353 into 500–10,000 L vertical storage tanks and transport vessels exposes the polymer to oven residence times of 25–45 min at set temperatures from 260°C to 315°C, conditions that make long-term thermal stabilization and particle-size control more important than melt-flow index alone. Articles intended for potable water service are certified to NSF/ANSI/CAN 61, and food-contact applications fall under FDA 21 CFR 177.1520. Rigid plastic intermediate bulk containers for dangerous goods are evaluated under UN 31H1 or UN 31H2 design type.
A typical dry blend contains 99.0–99.7 wt% D353, 0.05–0.15 wt% hindered phenolic antioxidant, 0.05–0.20 wt% UV stabilizer, and 2.0–3.0 wt% carbon black masterbatch for outdoor tanks. For water tanks, natural or white pigmentation at 1.0–2.0 wt% is used to minimize heat absorption. Biaxial rotational molding machines with a 4:1 rotational speed ratio are operated with oven air temperature set at 265–300°C. The cooling phase uses forced air followed by water mist; rapid surface cooling below 70°C increases warpage in flat-sided tanks, while excessively slow cooling extends cycle time without improving dimensional stability.
The narrow molecular weight distribution of metallocene MDPE reduces zero-shear viscosity compared with Ziegler HDPE, improving wall thickness uniformity in complex mold geometry but impairing bubble release. Trapped gas from moisture or outgassing of masterbatch carrier resin creates pinholes; pre-drying at 80°C for 2 h is required when storage relative humidity exceeds 60% and moisture content exceeds 0.02 wt%. Incompatible fluids include strong oxidizing acids, aromatic solvents, and halogenated hydrocarbons, which cause environmental stress cracking or swell distortion. Terminal products include vertical flat-sided storage tanks, conical bottom process tanks, inner bottles for rigid plastic IBCs, containment basins, and sewage holding tanks.
High-stalk blown film extrusion of D353 differs from conventional LLDPE film in that bubble stability is governed more by melt extension behavior and air ring configuration than by melt index alone. In 70–85 wt% blends with LDPE homopolymer at 15–30 wt%, the metallocene MDPE component reduces seal initiation temperature and improves dart impact and environmental stress crack resistance; however, the narrow molecular weight distribution lowers melt strength, so the process uses a high-stalk bubble with frost line height between 600 mm and 900 mm above the die.
Compliance for food-contact films is covered by FDA 21 CFR 177.1520 and EU Regulation 10/2011; REACH SVHC screening applies. The formulation consists of D353 70–85 wt%, LDPE 15–30 wt%, antiblock masterbatch 1.0–2.0 wt%, slip masterbatch 0.5–1.0 wt%, and polymer processing aid 0.5–1.0 wt%. For FIBC liners requiring surface resistivity 10⁹–10¹¹ ohm/sq per ASTM D257, 2.0–3.0 wt% amine-free antistatic masterbatch is added.
The line configuration includes a die gap of 1.8–2.4 mm, blow-up ratio 2.5:1–3.5:1, internal bubble cooling with air at 10–20°C, and melt temperature 190–225°C. Seal strength is measured per ASTM F88; hot-tack strength per ASTM F1921. Dart impact is determined by ASTM D1709 method B and tear resistance by ASTM D1922. Processing above 225°C increases gel formation, and lowering blow-up ratio below 2.5:1 reduces tear balance between machine and transverse directions. Terminal products include gusseted heavy-duty sacks, side-gusseted FIBC liners, dunnage air bags, form-fill-seal pouches for granular chemicals, and heavy-gauge industrial sheeting.
For UN-certified jerrican production, extrusion blow molding of 10–30 L jerricans and 60 L open-head drums from mPact D353 places a premium on parison melt strength, weld line integrity, and long-term environmental stress crack resistance in aggressive fill materials. The density of 0.933 g/cm³ reduces article mass compared with HDPE while still meeting UN performance certification for plastic jerricans under UN 3H1 and UN 3H2 designations. Dangerous goods packaging must pass the performance tests of 49 CFR 178.509, including drop at -18°C, leakproofness, hydrostatic pressure, and stacking. Food-contact containers are covered by FDA 21 CFR 177.1520.
The extrusion blow molding compound is 98–99 wt% D353, 1.0–2.0 wt% color masterbatch, and 0.5–1.0 wt% process aid. For outdoor storage, 2.0 wt% carbon black masterbatch is required. Total stearate lubricant loading is kept below 0.2 wt% because higher concentrations migrate to the mandrel/parison interface and reduce weld line strength. Shuttle-type accumulator extrusion blow molding machines with 20–40 point parison programming are operated at melt temperature 180–215°C, mold temperature 5–25°C, blow pressure 0.6–1.0 MPa, and cycle time 70–120 s. The extruder uses an L/D of 24:1–30:1 with barrier screw design and backpressure 15–25 MPa. A processing boundary exists below 1.2 mm wall thickness at the shoulder pinch-off, where -18°C drop-test failures increase sharply; top-load strength is verified per ASTM D2659 at not less than 1,500 N on an empty 20 L jerrican.
| UN test | Reference | Condition |
|---|---|---|
| Drop test | 49 CFR 178.603 | -18°C, multiple orientations |
| Leakproofness | 49 CFR 178.604 | 30 kPa, 10 min |
| Hydrostatic pressure | 49 CFR 178.605 | Per design type and fill material |
| Stack load | 49 CFR 178.606 | 40°C, 28 days |
Terminal products include UN-certified jerricans, open-head drums, automotive fluid containers, agricultural chemical packaging, and industrial liquid transport packagings.
Sheet extrusion of D353 for thermoformed containment products uses a flat die at 190–220°C melt temperature and a three-roll stack at 70–90°C to produce sheet thicknesses from 3.0 mm to 6.0 mm. The lower crystallinity of MDPE widens the thermoforming window relative to HDPE, but it also increases sag sensitivity above 160°C sheet surface temperature. Electronic handling trays used in manufacturing are evaluated against RoHS Directive 2011/65/EU for restricted heavy metals, and food-contact trays are covered by FDA 21 CFR 177.1520. Surface resistivity is characterized by ASTM D257.
The base formulation is 100 phr D353 with 1.5–3.0 wt% antistatic masterbatch for ESD-safe trays; UV-stabilized outdoor containment trays contain 2.0 wt% carbon black masterbatch. Thermoforming is performed at sheet surface temperature 130–160°C with plug-assisted forming using syntactic foam plugs, mold temperature 40–80°C, and forming pressure 0.3–0.7 MPa. Part warpage in flat-bottom trays is controlled by differential mold cooling; a temperature difference greater than 20°C between male and female mold surfaces causes measurable convex distortion. Terminal products include battery handling trays, chemical containment trays, automotive fluid catch basins, and dunnage pallet covers.
In extrusion coating of woven polypropylene substrates, mPact D353 is specified where low-temperature flexibility and flexural crack resistance during FIBC filling outweigh the higher coating stiffness of HDPE. The resin is processed at 260–310°C through a flat die with die gap 0.4–0.6 mm to deposit 15–30 µm coatings on 70–90 g/m² woven polypropylene fabric. Coated substrates for food contact are tested under FDA 21 CFR 177.1520 and EU Regulation 10/2011; REACH SVHC compliance applies.
The coating compound is 95–98 wt% D353, 2–5 wt% LDPE for neck-in reduction, and 0.5–1.0 wt% maleic anhydride-grafted adhesion promoter masterbatch. For moisture barrier lamination of chemical bags, 1.0–2.0 wt% process aid is added to reduce die build-up. The extrusion coating line runs at 100–300 m/min with an air gap of 100–200 mm and chill roll temperature 15–30°C. Neck-in must be held below 25 mm; melt draw resonance occurs when draw ratio exceeds 30:1. Adhesion to woven PP is measured by ASTM D1876 T-peel. Published data for this specific configuration with D353 is limited, so pilot trials are required to determine corona treatment level and adhesion promoter dosage. Terminal products include woven polypropylene bulk bag lamination, FIBC fabric coating, multiwall paper lamination, chemical bag moisture barrier layers, and flexible intermediate bulk container inner sheets.
Competitive Chevron Phillips mPact™ D353 m-MDPE Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chevron Phillips mPact™ D353 m-MDPE Linear Low Density Polyethylene is a metallocene-catalyzed ethylene-α-olefin copolymer supplied in pellet form. The resin is formally classified as a medium-density polyethylene under ASTM D883 because the nominal density lies within the 0.926–0.940 g/cm³ density band. The linear low-density nomenclature that appears in some supply-chain records refers to the linear molecular backbone and the absence of long-chain branching, not to a density below 0.925 g/cm³. Manufacturer technical literature lists a nominal density of approximately 0.933 g/cm³ tested in accordance with ASTM D1505 and a nominal melt index of approximately 5.0 g/10 min tested at 190 °C under 2.16 kg load in accordance with ASTM D1238 and ISO 1133-1:2022. The melt index places the product at the higher-flow end of the medium-density mPact range, making it suited to rotationally molded chemical tanks, industrial containers, large-part blow molding, and sheet extrusion where the flow rate must balance against sag resistance.
On a molecular level, the single-site catalyst produces a narrow molecular weight distribution and a more homogeneous short-chain branch distribution than is obtained using conventional Ziegler-Natta chemistry. High-temperature gel permeation chromatography under ISO 16014-4 or ASTM D6474 typically shows a polydispersity index below 2.5 for this grade family. The narrow distribution increases tie-molecule concentration at equivalent density. The practical consequence is that environmental stress crack resistance tested under ASTM D1693, condition B, can exceed 1,000 h without the density reduction that would otherwise lower flexural modulus. A representative flexural modulus of approximately 620 MPa under ASTM D790 is reported for the medium-density range. These values are nominal rather than lot-to-lot release limits, and the current grade-specific technical data sheet should be consulted for exact specification windows.
Melt rheology differs from autoclave high-pressure LDPE in one important respect: the metallocene linear architecture exhibits less shear thinning. At a given melt index, the D353 melt retains a higher apparent viscosity at high shear rates and a lower melt tension in extension. Blown-film and sheet-extrusion operations may therefore observe better gauge uniformity at high shear rates but more bubble flutter and draw sag than with a long-chain-branched LDPE of equivalent melt index. Die-lip plate-out is generally reduced because the metallocene catalyst leaves lower catalyst residue and the narrow composition distribution reduces the low-molecular-weight species that migrate to metal surfaces.
Melt fracture is not usually the limiting defect for D353 at conventional film and sheet shear rates. At die wall shear rates above 1,000 s⁻¹, sharkskin can appear on blown-film surfaces if the die-lip temperature is below 190 °C. The onset is controlled by raising the die-lip temperature to 200–220 °C or by using a fluoropolymer processing aid addition of 200–400 ppm. Processing aid effectiveness is reduced by the narrow composition distribution if the aid is added before the compression zone; the preferred injection point is after pellet melting.
Temperature control below 240 °C is the principal processing boundary. The resin can be processed on single-screw extruders with screw diameters from 45 mm to 90 mm and 24:1 to 30:1 L/D. A reverse temperature profile is typical, with the feed throat maintained below 180 °C, the feed zone between 160 °C and 175 °C, the compression zone between 180 °C and 205 °C, and the die head between 190 °C and 220 °C. Feed-throat bridging can occur when the rear barrel zone exceeds 180 °C because pellet softening advances into the solids-conveying section. Melt temperature at the die above 240 °C is not recommended because oxidative gel formation and taste-and-odor contributions increase rapidly beyond that threshold.
On grooved-feed extruders, pressure build-up with metallocene MDPE is more rapid than with high-pressure LDPE. A grooved barrel section length of 3–4 D and groove depth of 0.3–0.4 mm are common, but excessive backpressure can raise melt temperature above 230 °C and reduce output stability. Discharge pressure should be monitored and kept below 300 bar to avoid excessive screw wear and energy input.
For blown film, a die gap of 1.5–2.5 mm, a blow-up ratio of 2.5:1 to 3.5:1, and a frost-line height of 8–12 die diameters provide a stable starting window. The lower melt tension of the linear metallocene resin requires smaller draw ratios or adjusted air-ring settings to avoid bubble instability when output exceeds 8 kg/h per cm of die circumference. Film dart impact measured under ASTM D1709 is sensitive to frost-line position; excessively high frost lines can reduce transverse-direction impact by permitting over-orientation before crystallization.
In rotational molding, D353 is pulverized to a typical sieve size of 35 mesh (500 µm). Oven air temperatures between 260 °C and 320 °C and peak internal air temperatures of 200–220 °C are standard for medium-density parts. Demolding below 70 °C and controlled cooling rates of 4–8 °C/min minimize warpage and residual stress. Under-curing is indicated by inner-surface porosity and reduced solvent resistance; over-curing is identified by yellowing and a brittle skin layer. Published data for optimized D353 rotational-molding cycle times is limited and should be established on the specific mold geometry because wall thickness distribution depends on mold arm speed ratio and oven air circulation.
| Measurement | Test method | mPact D353 representative value | Conventional Ziegler-Natta MDPE comparison range |
|---|---|---|---|
| Density | ASTM D1505 | 0.933 g/cm³ | 0.934–0.940 g/cm³ |
| Melt index | ASTM D1238, 190 °C/2.16 kg | 5.0 g/10 min | 2.0–8.0 g/10 min |
| Flexural modulus | ASTM D790 | 620 MPa | 500–800 MPa |
| Tensile yield strength | ASTM D638 | 16 MPa | 14–20 MPa |
| ESCR, F50 | ASTM D1693, condition B | >1,000 h | 200–1,000 h |
| Brittleness temperature | ASTM D746 | <-75 °C | -20 to -60 °C |
The matrix is compiled from producer technical literature and typical Ziegler-Natta MDPE ranges reported in industrial references. Specimen preparation under ASTM D4703 or ISO 293 can shift individual values by several percent. The table is not a specification and should not replace the supplier’s certificate of analysis.
D353 differs from conventional Ziegler-Natta MDPE most strongly in ESCR retention. A Ziegler-Natta resin of comparable modulus may reach only 200–1,000 h under ASTM D1693, condition B, unless density is reduced toward 0.925 g/cm³. The metallocene architecture of D353 allows >1,000 h at a nominal density near 0.933 g/cm³. For rotationally molded chemical tanks and agricultural spray vessels, that difference allows wall thickness and top-load stiffness to be preserved while retaining resistance to stress cracking from wetting agents, detergents, and weak solvents.
Compared with high-pressure LDPE, the linear D353 backbone provides a higher crystalline melting point in the 120–125 °C range by ASTM D3418 differential scanning calorimetry and a higher flexural modulus. However, the absence of long-chain branching reduces melt elasticity. On blow-molding machines calibrated for LDPE, parison programming and die gap must be adjusted to avoid excess sag. Compared with butene-based LLDPE, the comonomer type and metallocene distribution in D353 produce a more effective tie-molecule network; low-temperature impact and ESCR generally improve, but film haze may increase slightly unless extrusion temperatures and blow-up ratios are optimized.
Industrial applications reported for the mPact medium-density family include agricultural chemical tanks, water storage cisterns, material-handling bins, insulated transport containers, and double-wall fuel containment components. The D353 melt flow rate is suited to thick-walled parts of 3–10 mm in rotational molding and sheet thickness of 2–6 mm by flat-die extrusion. In sheet thermoforming, the resin’s narrow molecular weight distribution provides a wider processing window for plug-assisted forming; however, sheet orientation must be controlled by maintaining uniform sheet temperature within ±5 °C across the forming window.
At density below 0.925 g/cm³, the flexural modulus of the resin family falls sharply because the crystalline fraction decreases nonlinearly. At density above 0.940 g/cm³, low-temperature impact and ESCR are sacrificed. The D353 design point near 0.933 g/cm³ avoids these two property cliffs while maintaining the required stiffness for large storage tanks. This balance is more sensitive to short-chain branch distribution than to average molecular weight; increasing melt index without modifying comonomer content can reduce ESCR rapidly.
Polyethylene grades in this density class are typically evaluated for food-contact suitability under 21 CFR 177.1520(c) and for European migration under EU 10/2011 when all additive and migration limits are satisfied. Because final part formulations may contain masterbatch, regrind, or processing aids, the converter is responsible for end-use compliance testing under the actual contact conditions. The grade is not formulated with heavy-metal pigments or brominated flame retardants that would normally trigger RoHS restrictions; REACH candidate-list SVHC status should be confirmed against the supplier’s current declaration.
For outdoor tanks and industrial containers, long-term performance is controlled by creep modulus under ASTM D2990, tensile property retention after weathering under ASTM D2565, and ESCR under ASTM D1693. The grade can be stabilized with carbon black or ultraviolet stabilizers by the converter; unstabilized natural resin is not suitable for extended direct sunlight. Published data specific to D353 in pressure-piping service is limited, and the product is not designed primarily for ASTM D3350 pressure-pipe cell classification. In non-pressure storage, the resin’s ESCR and modulus balance is the more relevant specification basis.
Pre-drying is not normally required for pellets or powder stored under dry indoor conditions. If the material has been exposed to condensation or relative humidity above 60%, a hopper dryer at 70 °C for 1 h is sufficient to remove surface moisture. Avoid blending with polypropylene or high-viscosity process oils above 2 wt%, because immiscible domains reduce impact strength and can cause delamination at knit lines. Clean edge trim and rejected parts may be reprocessed at addition levels up to 20 wt% provided the regrind is free of contamination and has not been thermally degraded; repeated extrusion above 240 °C should be avoided.