| HS Code | 527915 |
| Density | 0.914 g/cm³ |
| Melt Index | 0.9 g/10 min at 190°C/2.16 kg |
| Melt Flow Ratio | 16 |
| Melting Point | 119°C |
| Vicat Softening Point | 94°C |
| Tensile Strength At Yield | MD 1200 psi / TD 1100 psi |
| Tensile Strength At Break | MD 5000 psi / TD 4500 psi |
| Elongation At Break | MD 600% / TD 700% |
| 1 Secant Modulus | MD 24000 psi / TD 28000 psi |
| Dart Drop Impact | 250 g |
| Elmendorf Tear Strength | MD 150 g / TD 400 g |
| Haze | 5% |
| Gloss | 75% |
| Coefficient Of Friction | 0.2 |
| Comonomer | Hexene |
| Catalyst Type | Metallocene |
| Resin Type | Linear Low Density Polyethylene (LLDPE) |
As an accredited Chevron Phillips Marlex® D143FK Metallocene Linear Low Density Polyethylene, Blown Film factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 25 kg (55 lb) polyethylene bags, palletized, with optional bulk bags or bulk truck/railcar shipments. |
| Container Loading (20′ FCL) | Chevron Phillips Marlex® D143FK loads 24.75 MT net per 20′ FCL: 25 kg bags, 55 bags/pallet, 18 pallets, shrink-wrapped. |
| Shipping | Shipped as non-hazardous polyethylene resin pellets in 25-kg bags, octabins, or bulk trucks/railcars. Transport and store in a cool, dry, ventilated area away from moisture, heat, ignition sources, and sunlight. Keep packaging sealed to prevent contamination. No special DOT/IMDG placards required; consult SDS and local regulations. |
| Storage | Store Chevron Phillips Marlex® D143FK in a cool, dry, well-ventilated area, preferably indoors. Protect from direct sunlight, moisture, heat, sparks, flames, and oxidizing agents. Keep original bags/containers sealed and off the floor. Avoid dust generation and static discharge. Rotate stock first-in, first-out; observe shelf life and SDS recommendations. Do not store near incompatible materials. Ensure adequate ventilation. Follow all local regulations. |
| Shelf Life | Stable under normal storage; recommended shelf life: 12 months from manufacture in unopened original packaging, cool, dry, away from sunlight. |
In blown film extrusion of metallocene linear low density polyethylene, the manufacture of direct food contact films from Marlex D143FK follows a narrow window between melt temperature and frost line position. The resin is supplied as a hexene copolymer with a nominal density of 0.916 g/cm³ per ASTM D1505 and a nominal melt index of 1.0 g/10 min per ASTM D1238 at 190 °C/2.16 kg. Where the grade-specific technical datasheet reports different values, the datasheet governs. The resin can be processed on monolayer blown film lines using a die gap of 1.5 mm to 2.5 mm and a blow-up ratio of 2.0:1 to 2.5:1. Frost line height is maintained at 6 to 10 die diameters to avoid excessive machine-direction orientation and loss of transverse-direction tear. Melt temperature at the die is typically held between 190 °C and 230 °C; sustained operation above 230 °C may generate oxidative gel particles and reduce dart impact retention after regranulation. When direct food contact films are converted on high-speed form-fill-seal lines, a slip agent masterbatch based on erucamide or oleamide is added at 2 wt% to 5 wt% to achieve a kinetic coefficient of friction below 0.30 per ASTM D1894. Silica-based antiblock concentrate is dosed at 2 wt% to 4 wt% when blocking occurs on rewind. Fluoropolymer polymer processing aid addition at 200 ppm to 800 ppm is permissible for sharkskin suppression; however, its migration potential in monolayer food contact structures must be verified under the applicable regulatory framework. Direct food contact films produced from ethylene-hexene copolymers are evaluated under FDA 21 CFR 177.1520(c), and for the European Union they must meet the substance-specific and overall migration limits of EU Regulation (EU) No 10/2011. The converter is responsible for verifying that the additive package does not exceed the relevant specific migration limits listed in Annex I of EU 10/2011. The resulting monolayer films are converted into fresh produce bags, bakery carton overwrap, and thin frozen food bags. Continuous service above 80 °C is not recommended for monolayer polyethylene sealant films without package design modification.
| Region | Standard | Clause / method | Verification requirement |
|---|---|---|---|
| United States | FDA 21 CFR 177.1520(c) | Olefin polymer food additive regulation | Resin must be produced with authorized olefin comonomers; the converter must ensure that no unlisted processing aid migrates to food at levels exceeding applicable thresholds. |
| European Union | EU Regulation (EU) No 10/2011 | Annex I authorized substances; Article 17 migration limits | Overall migration limit 10 mg/dm² using food simulants assigned under Annex III; specific migration limits apply to slip, antiblock, and polymer processing aid additives. |
| China | GB 4806.7-2016 | Food contact plastic materials and articles | Overall migration limit 10 mg/dm²; potassium permanganate consumption and heavy metal migration per applicable clauses of the standard. |
| Japan | MHLW Notification No. 370 | Specifications for polyolefin food contact materials | Cadmium and lead content in the material are limited to 100 ppm each; migration testing is performed according to official methods. |
Marlex D143FK is blended into heavy-duty sack formulations at 70 wt% to 90 wt% with a high-pressure LDPE grade to raise melt strength and bubble stability. The LDPE grade selected for this purpose typically has a melt index of 0.25 g/10 min to 0.80 g/10 min and a density of 0.923 g/cm³ to 0.926 g/cm³. Film structures from 50 µm to 150 µm are produced on high-stalk or long-stalk blown film lines. Die gap is set at 2.0 mm to 2.5 mm, and the blow-up ratio is held between 2.2:1 and 3.0:1. The bubble is stabilized by a frost line height of at least 8 die diameters. Dart impact is evaluated per ASTM D1709 Method A or Method B depending on film thickness, and Elmendorf tear is measured per ASTM D1922. The addition of LDPE improves melt strength but can reduce dart impact relative to a neat D143FK film. Published data for this specific blend configuration is limited; the converter should run a design of experiments covering LDPE content, blow-up ratio, and frost line height before qualifying a commercial sack structure. If dart impact must remain above 400 g per ASTM D1709 Method A at 100 µm, LDPE addition is typically constrained to 10 wt% to 15 wt%. The lower melt strength of metallocene LLDPE is managed by using a barrier screw with L/D from 24:1 to 30:1 and a low-shear mixing section. Gauge bands and bubble instability are the primary failure modes observed on production-scale lines when the frost line is set too low or when the die lip pressure is insufficient. End products include 25 kg chemical sacks, flexible intermediate bulk container liners, industrial box liners, and construction film.
For thin-gauge elastic recovery applications, the processor should evaluate the film at 15 µm to 25 µm gauge. Blown film lines with a die gap between 1.5 mm and 2.0 mm and a blow-up ratio of 2.5:1 to 3.0:1 can produce a film with higher transverse-direction tensile strength than cast alternatives. The resin is combined with 5 wt% to 20 wt% of an ULDPE or plastomer having a melt index below 1.0 g/10 min and a density below 0.915 g/cm³ to increase puncture resistance and elastic recovery. Elongation at break is measured per ASTM D882 and puncture resistance per ASTM D5748. A tackifier such as polyisobutylene is added only when cling is required; for stretch hood applications, no cling additive is used. The film relies on elongation and recovery to secure the pallet after application. Processing on a high-blow-up-ratio bubble increases molecular orientation in the transverse direction, but the melt temperature must remain between 190 °C and 220 °C to avoid loss of extensibility. Published data for this specific D143FK configuration is limited; a trial program should include a design of experiments covering blow-up ratio, frost line height, and output rate. The terminal products are pallet stretch hoods, hand stretch film, and machine stretch film for logistics.
Agricultural film lines running D143FK require UV stabilizer masterbatch addition from 3 wt% to 5 wt%. The stabilizer system is selected from high-molecular-weight hindered amine light stabilizers and a UV absorber such as a benzotriazole or triazine. The masterbatch carrier resin should have a melt index within 0.5 g/10 min of the base resin to avoid melt flow disturbance. Greenhouse covers are produced at 100 µm to 200 µm in monolayer or three-layer blown film lines. The die gap is set at 2.0 mm to 2.5 mm, and the blow-up ratio is increased to 2.5:1 to 3.5:1 to improve transverse-direction tear and wind stability. For silage stretch film, thickness is reduced to 25 µm to 35 µm and the film is formulated with an anti-tack additive because the surface is wound under high tension. Tensile strength retention after artificial weathering is measured per ISO 4892-2. Agricultural films are not subject to direct food-contact migration limits, but REACH Annex XVII restrictions apply to cadmium, lead, and phthalates; the formulation should not include substances on the ECHA Candidate List above 0.1 wt%. Pre-drying is not required for internal moisture; if surface condensation is present after outdoor storage, a hopper dryer at 60 °C for 4 h is sufficient. Terminal products include greenhouse covers, mulch films, silage stretch film, and temporary crop protection sheeting.
On vertical form-fill-seal and horizontal form-fill-seal lines, the sealant layer must reach an acceptable seal strength below 100 °C to allow jaw dwell times below 0.3 s. Marlex D143FK is used as a sealant layer at 15% to 25% of total film thickness in coextruded blown structures. In a 75 µm structure, a 12 µm to 18 µm sealant layer is paired with an HDPE skin layer, an EVOH barrier layer, and a tie layer. The seal initiation temperature of metallocene LLDPE is lower than that of conventional LDPE; hot tack strength is tested per ASTM F1921 Method B, and seal strength is tested per ASTM F88/F88M. The sealant layer extrusion temperature is set between 200 °C and 220 °C. This is a process conflict when EVOH is coextruded because the EVOH layer must remain below 230 °C to avoid gel formation and black specks. The practical melt temperature range for the D143FK layer in these structures is therefore 190 °C to 220 °C. If the sealant layer is raised above 230 °C to improve adhesion, degradation in the adjacent barrier layer may occur. The converter should not use high levels of migratory erucamide in sealant layers that contact tie resins, because migration to the interlayer reduces adhesion. End products include frozen vegetable packaging, dairy pouches, processed meat films, and medical device pouches where a low-temperature seal is required.
Corona-treated blown sealant webs based on D143FK are laminated to biaxially oriented polypropylene, polyester, or aluminum foil for pouch constructions. The sealant web is produced at 25 µm to 50 µm and corona treated to a surface energy of 38 mN/m to 42 mN/m per ASTM D2578. Treatment is performed in-line before winding. The film is stored for no more than 3 months before lamination because corona treatment decay reduces adhesion. A solventless two-component polyurethane adhesive is applied at 1.5 g/m² to 2.5 g/m²; the sealant web must be free of migratory slip additives in excess of 0.5 wt% or bond strength measured per ASTM F904 may fall below 2 N/15 mm after 7 days. The use of an antiblock-only formulation is preferred for lamination sealant webs because erucamide migration to the treated surface reduces interlaminar adhesion. End products include stand-up pouches, liquid packaging, pet food bags, and non-food industrial pouches.
Competitive Chevron Phillips Marlex® D143FK Metallocene Linear Low Density Polyethylene, Blown Film prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chevron Phillips Marlex® D143FK is a metallocene-catalysed linear low density polyethylene resin formulated for blown film extrusion. The nominal density is 0.918 g/cm³ and the nominal melt index is 1.0 g/10 min at 190°C under 2.16 kg load, determined according to ASTM D1238 or ISO 1133-1:2022. The resin is supplied as pellets with a thermal stabiliser package. D143FK belongs to a metallocene product class characterised by lower heat seal initiation temperature, higher dart impact strength at equivalent film density, and reduced optical haze compared with conventional Ziegler-Natta linear low density polyethylene. End-use applications include high-speed form-fill-seal pouches, frozen food packaging, liquid packaging, clear overwrap, and heavy-duty shipping sacks. In coextruded constructions, the resin is applied as a sealant skin or as a toughness layer adjacent to EVOH or polyamide. Unlike autoclave LDPE, D143FK does not carry substantial long-chain branching; melt strength and bubble stability are therefore lower and must be controlled through die geometry, air-ring settings, and melt temperature.
The metallocene catalyst system used for D143FK produces a narrower molecular weight distribution and a more uniform short-chain branching distribution than heterogeneous Ziegler-Natta LLDPE. In conventional Ziegler-Natta resins, comonomer is incorporated disproportionately into lower molecular weight fractions. This leaves higher-density, low-branch species that raise seal initiation temperature and create larger crystalline domains that scatter light. D143FK reduces those populations. The result is a narrower melting range, lower seal bar temperature for load-bearing enclosure formation, and improved optical clarity on blown film lines. The reduction in high-density fractions also lowers stiffness slightly at equivalent density, but this is offset by improved dart drop impact as measured by ASTM D1709A. Thermally fractionated films show a smaller population of high-density crystallites than conventional LLDPE, and the melting peak is typically observed near 121°C to 123°C by ASTM D3418. The exact second-heat peak shifts with cooling rate and film thermal history.
Rheological fingerprints from parallel-plate oscillatory shear at 190°C show a broader Newtonian plateau than conventional Ziegler-Natta LLDPE and lower shear thinning than autoclave LDPE. The crossover frequency of storage modulus and loss modulus is lower in melt elasticity than long-chain-branched LDPE, consistent with the absence of long-chain branching. On a blown film line, this architecture reduces memory effect at the die exit but also reduces bubble tension. The frost line height has direct consequences for secondary crystallisation. A high frost line allows more ordered lamellae to form, increasing modulus while reducing clarity and dart impact. A low frost line retains a higher proportion of amorphous chain entanglements at the freeze point, improving impact and haze but lowering tensile modulus. The response to frost line position is often more pronounced in metallocene LLDPE than in conventional Ziegler-Natta LLDPE because the uniform branching distribution reduces the less branched fraction that otherwise provides stiffness and melt structural integrity. The comparatively low extractable content is relevant to organoleptic and food-contact uses; solvent extraction data are normally supplied in the manufacturer’s regulatory documentation.
Extrusion of D143FK on a 60 mm to 90 mm groove-fed extruder with 25:1 to 30:1 L/D requires careful screw design and screen-pack selection. Because the molecular weight distribution is narrow, the resin retains higher viscosity at high shear than LDPE of equivalent melt index. Die pressure and motor load therefore respond more steeply to screw speed. Typical conditions use melt temperatures of 190°C to 220°C, die gaps of 1.0 mm to 2.0 mm, and blow-up ratios of 2.0:1 to 3.0:1. For a 25 µm film, the frost line is generally maintained below 300 mm from the die face when high clarity is required. Higher frost lines allow greater crystallinity but may reduce gloss and impact strength. If gauge uniformity is outside ±5%, manual adjustment of the air-ring lip or internal bubble cooling is required; automatic gauge control with segmented air rings reduces long-term variation across the web.
Metallocene LLDPE can develop sharkskin melt fracture at lower critical shear rates than LDPE. The exact onset is die-geometry dependent, but the use of a fluoropolymer-based processing aid at 200 ppm to 600 ppm is common to extend the output window. On a 90 mm groove-fed line with a 1.5 mm die gap, output is typically limited by bubble stability rather than by plastication. Chilled air at 5°C to 15°C improves heat removal and bubble stiffness. The melt temperature at the die exit should generally not exceed 230°C to avoid oxidative gel formation. In high-output operation, the bubble-stability cage is set for a blow-up ratio of 2.0:1 to 2.5:1; incorrect cage contact can distort the bubble and generate gauge bands. Batch-to-batch melt index variation should be monitored with ISO 1133-1:2022 because thin-gauge film control is sensitive to viscosity drift.
In coextruded structures, D143FK is commonly placed as an external sealant skin on substrates of high-density polyethylene, polypropylene, or ethylene vinyl alcohol. Heat seal performance is evaluated on a laboratory heat sealer with 0.5 s dwell time and 2.75 bar sealing pressure. Films with a D143FK sealant layer typically generate seal initiation temperatures below 100°C when measured according to ASTM F88/F88M. Hot tack strength is assessed according to ASTM F1921. The low seal initiation temperature is valuable in vertical form-fill-seal packaging where high packaging speeds require rapid seal development and controlled seal-through-contamination behaviour. Reports should include seal temperature, seal pressure, dwell time, and failure mode; a single peel force without these conditions is insufficient for source qualification. In frozen food applications, impact strength is evaluated after conditioning specimens at -20°C; failure mode is reported as ductile or brittle according to ASTM D1709A. Published data for this specific configuration is limited, but the metallocene comonomer distribution generally confers better low-temperature dart impact than butene-based Ziegler-Natta LLDPE of identical density.
In a multilayer film containing EVOH or polyamide, the total melt temperature at the die exit should generally be maintained between 210°C and 225°C to preserve tie-resin performance without degrading the barrier polymer. Interfacial adhesion between D143FK and an anhydride-modified tie resin depends on melt temperature and interfacial contact time. Excessive temperature can generate EVOH gel formation, while insufficient temperature can reduce interfacial strength. Line purging between structures should be performed with LDPE or a dedicated purge compound. D143FK can also be used as the sealant web in adhesive laminations to PET or BOPP; seal strength is measured by pulling the seal at 90° to the seal direction using ASTM F88/F88M. Hot tack performance according to ASTM F1921 is used to predict seal integrity before the seal cools. A resin with low seal initiation and high hot tack reduces leaker rates in form-fill-seal operations. The low extractable content of metallocene LLDPE may provide organoleptic advantages in liquid packaging, but suitability must be confirmed by migration testing on the finished structure.
Replacement of autoclave LDPE with D143FK on a line originally designed for high-pressure LDPE can destabilise the tubular bubble because D143FK has lower melt strength and does not exhibit the same extensional strain hardening. The high stalk characteristic of LDPE cannot be transferred directly; a lower stalk height and a smaller die gap reduce the unsupported melt area. Processors should evaluate air-ring velocity. High-velocity air at excessive throw height can induce bubble oscillation and gauge variation. Reducing blow-up ratio from 2.5:1 to 2.0:1 and reducing melt temperature toward 190°C raises melt viscosity and improves bubble stiffness. Conversely, when D143FK replaces conventional Ziegler-Natta LLDPE, the narrow molecular weight distribution reduces shear thinning, so die head pressure may rise by 5% to 15% at constant screw speed. Rear-zone barrel temperatures can be set 5°C to 10°C higher to improve solids conveying, but excessive transition-zone temperature can lower melt density and create surging.
The lower melt strength of D143FK restricts output when the air ring delivers high-velocity air at excessive throw height. One production-scale response is to add fluoropolymer processing aid at 200 ppm to 600 ppm before increasing die gap. A larger die gap may reduce drawdown and degrade transverse direction tear; processing aid additions should be attempted first because they reduce die-pressure build-up without altering the drawdown ratio. Conversion from Ziegler-Natta LLDPE to D143FK may also require lowering the frost line from the original set point to maintain clarity and impact strength. If internal bubble cooling is installed, the stabilisation cage should be repositioned to match the lower stalk height; failure to reposition can create temperature asymmetry and variable film gauge. The ideal combination on fixed-air-ring lines is usually a lower BUR, moderate frost line, and melt temperature near 190°C to 210°C. Published data for this specific configuration is limited, but the operational boundary is defined by the interaction between melt strength and cooling capacity rather than by plastication capacity.
The following typical values are drawn from the manufacturer’s general product information and monolayer film evaluations. They are not specification limits and vary with blow-up ratio, frost line height, die gap, gauge, and line configuration.
| Property | Test Method | Typical Value or Range |
|---|---|---|
| Density | ASTM D1505 | 0.918 g/cm³ |
| Melt index, 190°C/2.16 kg | ASTM D1238 / ISO 1133-1:2022 | 1.0 g/10 min |
| Melting temperature | ASTM D3418 | 121°C to 123°C |
| Vicat softening temperature | ASTM D1525 | 96°C to 100°C |
| Dart drop impact, 25 µm film | ASTM D1709A | 250 g to 450 g |
| Elmendorf tear, MD/TD, 25 µm film | ASTM D1922 | 150 g to 300 g / 250 g to 450 g |
| Haze, 25 µm film | ASTM D1003 | 5% to 12% |
| Gloss, 45° | ASTM D2457 | 55 to 80 |
| Attribute | D143FK mLLDPE | Conventional ZN LLDPE | Autoclave LDPE |
|---|---|---|---|
| Catalyst system | Metallocene single-site | Ziegler-Natta multi-site | Free-radical high-pressure |
| Short-chain branching distribution | Uniform | Heterogeneous | Highly branched with long-chain branching |
| Seal initiation temperature | Lower | Intermediate | Higher |
| Dart impact at comparable density | High | Moderate | High |
| Haze by ASTM D1003 | Low | Moderate | Low to moderate |
| Melt strength | Low to moderate | Moderate | High |
| Extruder back pressure at equivalent melt index | Higher than LDPE | Higher than LDPE | Lower |
Material handling of D143FK follows standard polyethylene practice. Pre-drying is not required for normal dry storage. If surface condensation is present, the resin should be equilibrated in a dry area above dew point before extrusion. Prolonged exposure to ultraviolet light can cause photooxidative chain scission; the resin should be stored in closed packaging away from direct sunlight. Regrind can be reintroduced at controlled levels, but high levels of reworked film can increase gel formation and reduce dart impact. The melt index should be checked after repeated extrusion cycles; large increases in melt index after recycling may indicate excessive thermal degradation. Film can be surface treated by corona discharge. Typical surface energy targets for printing or lamination are 38 dyn/cm to 42 dyn/cm, equivalent to 38 mN/m to 42 mN/m. Corona treatment level decays with time and should be confirmed immediately before converting.
For food-contact applications, the finished film must comply with applicable end-use requirements. Olefin polymers are referenced in 21 CFR 177.1520 in the United States. Compliance is not a property of the resin alone; it depends on the additive package and the extraction performance of the finished article. In the European Union, plastic materials and articles are regulated under EU Regulation 10/2011 with an overall migration limit of 10 mg/dm² for most applications or 60 mg/kg for certain packaging conditions. Specific conformity test data should be obtained from the resin supplier or measured on the finished structure. D143FK is not intended for pharmaceutical or medical implant use; such applications require separate regulatory documentation and validation.