| HS Code | 185738 |
| Melt Index | 0.9 g/10 min |
| Density | 0.918 g/cm³ |
| Melting Point | 119 °C |
| Vicat Softening Point | 95 °C |
| Tensile Strength At Break Md | 5,500 psi |
| Tensile Strength At Break Td | 5,000 psi |
| Elongation At Break Md | 500% |
| Elongation At Break Td | 600% |
| Elmendorf Tear Strength Md | 250 g |
| Elmendorf Tear Strength Td | 500 g |
| Dart Drop Impact | 500 g |
| Haze | 6% |
| Gloss 45 | 70% |
| 1 Secant Modulus Md | 25,000 psi |
| 1 Secant Modulus Td | 28,000 psi |
As an accredited Chevron Phillips Marlex® D139DK Metallocene Linear Low Density Polyethylene, Blown Film factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg polyethylene-lined bags, forty bags per pallet, providing 1,000 kg net per pallet. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): Chevron Phillips Marlex® D139DK mLLDPE blown film resin in 25 kg bags, palletized, shrink-wrapped and secured. |
| Shipping | Chevron Phillips Marlex® D139DK is a non-hazardous metallocene LLDPE resin supplied as free-flowing pellets. It is shipped in 25 kg bags, 1,000 kg bulk bags on pallets, or bulk trucks/railcars. Store in a cool, dry, clean area away from heat, moisture, UV, and contaminants. Not regulated for transport. |
| Storage | Store Marlex D139DK in a cool, dry, well-ventilated area, in original sealed bags or packaging. Protect from direct sunlight, heat, moisture, sparks, flames, and strong oxidizing agents. Keep away from odors and contaminants. Use first-in, first-out rotation. Store at ambient temperature; keep packages closed when not in use. Avoid unprotected outdoor storage. |
| Shelf Life | Shelf life is typically 12 months from date of manufacture when stored unopened in original packaging under cool, dry conditions. |
In frozen-food vertical form-fill-seal operations, D139DK—a metallocene ethylene-hexene LLDPE with density 0.918 g/cm³ per ASTM D1505 and melt index 1.0 g/10 min at 190°C/2.16 kg per ASTM D1238—is converted into heat-seal webs where low-temperature seal initiation and hot-tack strength control leaker rates. The sealant layer in a three-layer structure typically contains 70–85 wt% D139DK and 15–30 wt% high-pressure LDPE film resin; the core uses a higher-stiffness LLDPE or HDPE, and the outer skin carries slip/antiblock masterbatch at 2–4 wt%. Extrusion on a grooved-feed extruder with L/D 30:1 and barrier screw is performed at melt temperature 195–215°C, die gap 1.4–2.0 mm, blow-up ratio 2.2:1 to 2.8:1, and frost-line height positioned at 3–5 die diameters to balance bubble stability and optical uniformity. Hot-tack force is measured per ASTM F1921, seal strength per ASTM F88, dart drop per ASTM D1709 Method A, and Elmendorf tear per ASTM D1922. Terminal articles include IQF vegetable pillow packs, seafood liners, ice cream bags, and pastry overwrap. The processing boundary is defined by gel sensitivity: melt temperatures above 220°C during extended residence increase oxidation gel counts, while pre-drying is not required below 60% RH.
| Jurisdiction | Regulation or standard | Test condition | Metric |
|---|---|---|---|
| United States | FDA 21 CFR 177.1520(c) 3.1 | Food-contact use conditions A through D | Extractives limits in fatty and aqueous simulants |
| European Union | EU Regulation 10/2011 | Migration into 10% ethanol, 3% acetic acid, 95% ethanol | Overall migration ≤ 10 mg/dm² |
| REACH | REACH Regulation (EC) No 1907/2006 | Candidate list screening | SVHC < 0.1 wt% |
Industrial heavy-duty sack constructions for minerals, resin pellets and chemical prills rely on a three-layer blown film in which D139DK is placed in the outer and inner skins while post-consumer recycled polyolefin occupies the core. A measurable layer distribution is 25 wt% outer skin, 45 wt% core, and 30 wt% inner skin; the outer skin may contain 10–20 wt% high-pressure LDPE to increase bubble stability, while the core may carry up to 50 wt% recycled LLDPE from internal converter scrap or rigid HDPE regrind, provided melt filtration through 120–200 μm screen packs is applied and sieve-based contaminant screening rejects rigid particles above 250 μm. The metallocene skin provides dart impact and low-temperature puncture resistance against sharp crystalline edges in mineral fillers. Extrusion uses a grooved-feed extruder with L/D 30:1 and barrier screw; skin-layer melt temperature is held at 200–220°C, die gap at 2.0–2.5 mm, and blow-up ratio between 1.8:1 and 2.4:1 because lower BUR preserves machine-direction impact orientation and reduces crease splitting at gusset folds. Heavy-duty sack film thickness normally falls between 100 μm and 180 μm, with gusseted layflat width up to 900 mm. Mechanical acceptance includes tensile strength at break per ISO 527-3, Elmendorf tear per ASTM D1922, and dart drop per ASTM D1709 Method A. Terminal sacks are closed by single-needle stitching or reinforced heat sealing. Packaging and Packaging Waste Directive 94/62/EC applies to the final article, with the sum of lead, cadmium, mercury and hexavalent chromium below 100 mg/kg; REACH Annex XVII restrictions apply to any imported recycled fraction. Operational limitations include increased bubble instability when the core layer contains more than 50 wt% variable-melt-index recycled film scrap, and extrusion pressure rise when screen packs capture black spec or gel agglomerates.
Silage conservation films require a minimum use life of 12 months under UV irradiation and acidic leachate exposure. D139DK is formulated with hindered amine light stabilizer masterbatch at 0.8–1.5 wt%, a benzophenone or benzotriazole UV absorber at 0.2–0.5 wt%, and, where opacity is required to reduce silage heating, rutile titanium dioxide at 2–4 wt%. The acid resistance of the polyethylene matrix avoids ester hydrolysis observed in some biodegradable films; this grade is intended for pit covers and bale wrap, not for soil-incorporable mulch. Extrusion uses a blow-up ratio of 2.5:1 to 3.0:1 and layflat between 4 m and 12 m; thickness for bale wrap ranges from 25 μm to 40 μm, while pit silage sheets can exceed 150 μm. Conformity under EN 13206 requires the film to survive artificial weathering per ISO 4892-2 with no visual cracks at the stated exposure interval; tensile retention is measured according to ISO 527-3 and tear resistance according to ISO 6383-2. Terminal products are round bale stretch films, clamp films, and mulching layers for silage piles. A processing boundary appears when the UV masterbatch carrier resin has a lower melt index than the base metallocene; if the carrier is external at 2.0–5.0 g/10 min, dispersion remains uniform, but high-viscosity carriers can produce optical gels and localized agglomerates of ≥50 μm that act as tear initiators. Drying is unnecessary below 60% RH; however, extended hot-air storage of masterbatch blends at 40°C can cause additive segregation.
Collation shrink lines for beverage multi-packs and food cans use a double-bubble process in which a primary tube is quenched, re-heated, and inflated to orient the film. D139DK is added to high-pressure LDPE at 20–40 wt% to raise dart impact and reduce seal initiation temperature, while the LDPE contributes the high shrink tension needed to hold bottle contours. In the primary extrusion step the melt temperature is held at 180–200°C because higher temperatures increase surface oxidation that suppresses reheat orientation in the secondary bubble. Die gap is set at 1.8–2.2 mm and primary BUR below 1.5:1; in the secondary bubble, stretch ratios are normally 4:1 in the machine direction and 4:1 in the transverse direction. Terminal film thickness is 30–50 μm for bottle multipacks and 50–70 μm for can overwrap. Shrink tension and percent shrink are measured per ASTM D2838; seal strength before and after shrinkage follows ASTM F88. Food-contact compliance for the overwrap is limited to indirect contact unless the final article is cleared under FDA 21 CFR 177.1520 and EU Regulation 10/2011. A critical limitation occurs when the D139DK fraction exceeds 40 wt%: the displacement of high-pressure LDPE reduces shrink force below the threshold required to hold a 12-pack PET bottle configuration without wrinkling. In addition, secondary-bubble dwell times above 120 s at reheat temperatures greater than 130°C can anneal the formed tube and lower final shrink.
Stand-up pouch converting lines require a blown sealant web that seals through product dust without losing hot-tack strength at 105–140°C. D139DK is extruded as a 50–70 μm monolayer or coextruded skin and laminated to oriented polyester, metallized polyester, or aluminium foil with a solventless polyurethane adhesive. The sealant layer is produced at melt temperature 195–210°C, die gap 1.2–1.6 mm, and blow-up ratio 2.0:1 to 2.4:1. For hot-tack improvement, up to 20 wt% high-pressure LDPE is introduced; replacement beyond that level compromises puncture roughness of the pouch side seal. Hot-tack strength is measured according to ASTM F1921, seal initiation temperature by ASTM F88, and caulkability by measuring seal strength through folded regions or gussets. The sealant web meets FDA 21 CFR 177.1520 and EU Regulation 10/2011 for fatty and aqueous foods when no intentional release of slip additives exceeds the stated specific migration limits. Terminal pouch types include dry pet food, frozen fruit, and non-retort snack pouches where the sealant remains below the retort ceiling and is not used as the sole barrier. A converter limitation is the interaction between the slip/antiblock package and lamination adhesion; erucamide migration to the laminate surface can reduce peel strength in some solventless polyurethane systems. Peel adhesion between the sealant and the barrier web is checked per ASTM F904 after 24 h aging at 50°C. Published data for D139DK hot-tack plateau width on high-speed pouch lines is limited; converters should establish the lower seal limit using statistically designed seal-bar pressure and dwell-time matrices.
Surface protection film for polished stainless steel and polycarbonate glazing uses D139DK as the stiff outer skin coextruded with a polyolefin plastomer tack layer. The outer skin contains antiblock masterbatch at 1–2 wt%; peel adhesion to 304 stainless steel is held between 0.1 N/25 mm and 0.8 N/25 mm when tested per ASTM D3330. After 6 months UV exposure at 50°C, the film must remove without adhesive transfer. RoHS 2011/65/EU and REACH SVHC content below 0.1 wt% apply for electrical-facing components. The application is limited to peel-force stability and optical inspection of the protected substrate; no additional mechanical test gates are routinely imposed.
The use of D139DK in cleanroom-blown sterile barrier overwrap requires validation that process-generated oxidation products and processing aids do not induce cytotoxicity. Film is extruded on a dedicated cleanroom line with HEPA-filtered cooling air and sealed folding frames, using melt temperature 190–210°C, die gap 1.8–2.0 mm, blow-up ratio 2.4:1 to 3.0:1, and thickness 50–75 μm. Sterile barrier compliance is assessed under ISO 11607-1:2019 for seal integrity and peelability; biological reaction follows ISO 10993-5:2009 for cytotoxicity and ISO 10993-10:2010 for sensitization and irritation. Extractables screening is often performed with 95% ethanol and water immersion at 40°C for 72 h, followed by gas chromatography-mass spectrometry and liquid chromatography-mass spectrometry; the final film must not release total organic carbon above the applicable USP 661.2 profile for plastic packaging systems. A production-scale risk is cross-contamination with erucamide slipping agent from adjacent coextruded lines; therefore the overwrap skid is purged for 4–6 h and verified by Fourier transform infrared spectroscopy before first-use lamination. The terminal articles are sterile peelable pouches, procedure kits, and device tray overwrap. Cleanroom operators record non-viable particulate counts per ISO 14644-1; films with surface defects larger than 0.5 mm in the seal area are rejected under ASTM F1886.
Competitive Chevron Phillips Marlex® D139DK Metallocene Linear Low Density Polyethylene, Blown Film prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chevron Phillips Marlex® D139DK is a metallocene-catalysed linear low-density polyethylene supplied for blown film conversion. The manufacturer-published nominal density is 0.918 g/cm³ when determined in accordance with ASTM D1505, and the nominal melt flow rate is 1.0 g/10 min under ASTM D1238 at 190 °C and 2.16 kg. These two characterization points place the resin in a low-moderate-density, low-melt-index envelope used where blown film toughness, sealability, and stress crack resistance are specified. The grade is not intended for injection moulding, extrusion coating, or blow moulding; its rheology and additive loading are directed to annular-die blown film processing. The condensed public datasheet does not fully disclose slip, antiblock, and stabilizer concentrations, so lot-specific certificates of analysis are required before release of converted film. Food-contact compliance is generally positioned within FDA 21 CFR 177.1520, with final migration and end-use compliance evaluated under EU Regulation 10/2011 where applicable.
| Property | Test method | Specification use |
|---|---|---|
| Density | ASTM D1505 | Nominal 0.918 g/cm³ for resin identity and film yield estimation |
| Melt flow rate | ASTM D1238 (190 °C/2.16 kg) | Nominal 1.0 g/10 min for lot consistency and extrusion pressure prediction |
| Dart impact | ASTM D1709 | Film toughness; value supplied on certificate of analysis or converter trial |
| Elmendorf tear | ASTM D1922 | Machine-direction and transverse-direction tear balance |
| Tensile properties | ASTM D882 | Yield and break values; gauge and orientation dependent |
| Haze and gloss | ASTM D1003, ASTM D2457 | Optical quality; dependent on die gap, blow-up ratio, and frost-line height |
| Seal initiation | ASTM F88, ASTM F2029 | Sealant-layer performance; line-specific trial required |
| Water vapour and oxygen transmission | ASTM F1249, ASTM D3985 | Barrier of final oriented film; structure-dependent |
Because density is fixed at 0.918 g/cm³, property differences arise primarily from molecular weight distribution, comonomer type and distribution, and additive loading. The exact comonomer type is not stated in the condensed datasheet; converters should not assume hexene or butene without supplier confirmation. The metallocene catalyst system produces a narrower molecular weight distribution and more uniform comonomer placement than a conventional Ziegler-Natta LLDPE of equivalent melt index. This shift alters shear-thinning behaviour, seal initiation, and melt elasticity. It does not, however, create a universal film property advantage. A broad-MWD Ziegler-Natta grade may exhibit greater melt strength and more forgiving bubble stability on older low-output lines, while D139DK trades part of that processing latitude for improved dart impact measured by ASTM D1709, improved tear resistance measured by ASTM D1922, and improved optical uniformity measured by ASTM D1003 and ASTM D2457 when cooling conditions are controlled. Stiffness measured by ASTM D882 is comparable to other 0.918 g/cm³ LLDPE grades; differences of 5–10% in tensile modulus can arise from orientation history rather than resin chemistry.
Relative to high-density polyethylene, D139DK has lower modulus and lower heat resistance. The 0.918 g/cm³ density reduces tensile yield stress measured by ASTM D882 compared with HDPE films of 0.950 g/cm³ or higher. Relative to high-pressure LDPE, D139DK lacks the same degree of long-chain branching, so it does not reproduce the strain-hardening and bubble stability of LDPE in heavy-wall films. It is not a fractional-melt film resin for geomembrane or a cast film resin; the 1.0 g/10 min melt flow rate is too low for typical cast film output and too high for very thick blown film requiring prolonged bubble residence. These boundaries define where the grade is technically separable from adjacent product families.
Metallocene catalysis shifts the molecular architecture away from the broad molecular weight distribution and heterogeneous comonomer placement typical of Ziegler-Natta LLDPE. In melt rheology, the practical consequence is lower low-shear viscosity relative to a Ziegler-Natta LLDPE of equivalent melt index, which can reduce die pressure but also reduce melt relaxation before the frost line. In film form, the conversion difference is usually visible in seal initiation and optical uniformity. A narrower comonomer distribution reduces the fraction of poorly dispersed comonomer-rich chains that contribute to high haze and low hot-tack. The trade-off appears in bubble stability: D139DK may require more deliberate selection of blow-up ratio, frost-line height, and die gap than a broader-MWD LLDPE when run at the same output. Published systematic comparisons of mLLDPE and Ziegler-Natta LLDPE show that the metallocene advantage is not absolute; line geometry and cooling intensity often determine whether the lower extractables and improved toughness become usable film properties.
In coextruded packaging structures where D139DK is placed as the sealant layer, the practical specification is often written around seal initiation temperature, hot-tack force, and coefficient of friction rather than density alone. Seal initiation is measured by ASTM F88 or ASTM F2029 and is sensitive to seal bar temperature, dwell time, pressure, and film gauge. A 25 µm monolayer film sealed at 120 °C under 0.3 MPa for 0.5 s may shift seal strength by more than 20% if frost-line height is altered; the resin datasheet cannot capture this conversion dependence. Typical end uses for mLLDPE in the 0.918 g/cm³ range include heavy-duty sacks, frozen food packaging, collation shrink film, and overwrap. In these structures, D139DK is used as a bulk or skin layer where the film must survive puncture by frozen product edges or package corners without requiring HDPE-level stiffness.
High-stalk extrusion of a 1.0 g/10 min mLLDPE with 0.918 g/cm³ density places a larger fraction of the total film gauge in the oriented section of the bubble than low-stalk LDPE. On a monolayer line equipped with a barrier screw of 24:1 to 30:1 L/D, a dual-lip air ring, and internal bubble cooling, the limiting process variable is usually bubble oscillation rather than motor load. The narrow molecular weight distribution reduces elastic recovery, so melt strain developed in the die land relaxes less before the frost line. If the die gap is reduced below 1.5 mm to improve clarity, die-lip shear stress increases and surface melt fracture can appear at high output. If the die gap is opened above 2.5 mm, the bubble may become harder to cool uniformly, increasing transverse gauge variation. A blow-up ratio between 2.0:1 and 2.5:1 is commonly selected, but the actual value must be trimmed to film width, frost-line height, and collapse-frame geometry.
Barrel temperature zones are usually set in the range 180–205 °C, with the adapter and die held near 205–220 °C to balance melt fracture and thermal degradation. Running the die too cold lowers melt strength; running it too hot raises the risk of oxidation at the die lip. At 220 °C, residence time at the die lip should be minimised by avoiding oversized die heads. Pre-drying is not required under normal ambient storage, but condensation on cold pellets introduced into a warm production area can create feed instability. Pellets should be brought to hopper ambient temperature before startup. The coefficient of friction measured by ASTM D1894 is controlled by the slip additive package; if the film is corona treated, coefficient of friction may increase over time as additive migration is altered. Published data for this specific formulation is limited; therefore, converter trials on the actual monolayer or coextruded line remain mandatory before specifying D139DK for a new package.
Seal initiation temperature in mLLDPE is influenced by polymer density, comonomer placement, and molecular weight distribution, but also by bubble cooling history. A lower density such as 0.918 g/cm³ reduces seal initiation relative to a 0.925 g/cm³ LLDPE, but the exact onset depends on film gauge, seal pressure, and dwell time. D139DK may be selected over a conventional LLDPE sealant when the package requires a lower seal initiation temperature without a reduction in dart impact. In vertical form-fill-seal operations, hot-tack force measured under ASTM F1921 can be more important than seal strength because the seal must resist product loading before full crystallization. If hot-tack is insufficient, the package opens at the seal; this failure is not predicted by melt flow rate or density alone. D139DK should not be compared directly to EVA or ionomer sealants for low-temperature seal performance. Those products have different polarity, density, and hot-tack envelopes. The metallocene LLDPE may provide lower extractables and better downgauging potential than some EVA sealants, but it is not a universal replacement for ionomer in high-abuse applications where seal-through-contamination is critical.
From a compliance standpoint, the grade is usually positioned within the olefin polymer class covered by FDA 21 CFR 177.1520(a)(3)(i) and EU Regulation 10/2011, but the final film must be evaluated for overall migration and specific migration limits because printing inks, adhesives, and coextruded layers contribute to the final composition. For medical packaging, converters may require ISO 10993 biological evaluation, but the resin supplier does not provide device-level certification. The absence of a complete monograph from the condensed datasheet means that lot-specific certificates of analysis are the only reliable basis for release testing.
On a coextruded heavy-duty sack line using D139DK as the skin layer over a high-density core, the primary observed defect is transverse gauge bands that form as the collapsing frame becomes worn or misaligned. Because the mLLDPE skin is less stiff than the HDPE core, small gauge reductions in the skin layer can localize elongation under drop impact. The relevant test is not a single resin property but the dart impact of the final coextruded structure under ASTM D1709, with film thickness measured at 10 mm intervals across the layflat to capture gauge bands. Converters running high-stalk conditions should record frost-line height, bubble internal pressure, and air-ring pressure before changing resin lots, because lot-to-lot variation in melt flow rate and slip additive can reproduce instability symptoms that are otherwise mistaken for equipment drift.