| HS Code | 541769 |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene |
| Melt Index 190 C 2 16 Kg | 1.0 g/10 min |
| Density | 0.918 g/cm³ |
| Melting Point | 122 °C |
| Vicat Softening Point | 100 °C |
| Tensile Strength At Yield | 1400 psi |
| Tensile Strength At Break | 4000 psi |
| Elongation At Break | 700 % |
| Flexural Modulus | 35000 psi |
| Dart Drop Impact | 200 g |
| Elmendorf Tear Md | 300 g/mil |
| Elmendorf Tear Td | 400 g/mil |
| Haze | 12 % |
| Gloss 45 | 60 % |
| Coefficient Of Friction | 0.2 |
As an accredited Chevron Phillips Marlex® 7120B LLDPE Blown & Cast Film Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Chevron Phillips Marlex® 7120B is packaged in 25 kg bags, 55 bags per pallet (1,375 kg total). |
| Container Loading (20′ FCL) | 20′ FCL: 25 kg bags, floor loaded; approximately 800 bags (20 MT) of Chevron Phillips Marlex® 7120B LLDPE Blown & Cast Film Resin. |
| Shipping | Marlex® 7120B LLDPE is non-hazardous and not DOT-regulated, typically shipped in 25 kg polyethylene bags on pallets—often 50 bags (1,250 kg) per pallet—or in bulk trucks/railcars. Keep packaging dry, sealed, and away from sunlight, moisture, and contamination during transport. |
| Storage | Store Chevron Phillips Marlex® 7120B LLDPE Blown & Cast Film Resin in a cool, dry, well-ventilated warehouse, using original sealed packaging. Keep pallets off the floor and away from direct sunlight, moisture, excessive heat, and ignition sources. Prevent contamination and excessive stacking. Rotate stock first-in, first-out. Follow the supplier’s safety data sheet and local regulations. Maintain normal ambient warehouse temperatures. |
| Shelf Life | Stable under normal storage; indefinite shelf life when kept cool, dry, away from direct sunlight and contaminants in original packaging. |
On a five-layer cast stretch line with a 2,800-mm die and a haul-off target of 350 m/min, Marlex 7120B is introduced into the core layers at 70–80 wt% blended with a 0.918 g/cm³ metallocene octene LLDPE at 20–30 wt%. The skin cling layers receive 1.5–3.0 wt% polyisobutylene in a low-density carrier resin, while the outer abrasion layer is formulated with 20 wt% LDPE to reduce roll blocking. Extrusion melt temperature is held between 240°C and 265°C, the die gap is set to 0.8 mm, and the chill roll temperature is maintained at 18–22°C with a dual air knife pressure of 6–10 kPa. At haul-off speeds above 400 m/min, neck-in increases and edge thickness variation exceeds ±8% unless the die lip heaters are trimmed; acceptable neck-in is kept below 30 mm per side. Compliance for pallet stretch wrap used as an indirect food transport aid is assessed under FDA 21 CFR 177.1520 for olefin polymers and under EU Regulation 10/2011 when the film is placed in direct contact with unpackaged food, with overall migration not exceeding 10 mg/dm² under the applicable food simulant migration test. Puncture propagation resistance is measured by ASTM D5748, stretch force by ASTM D5458, and coefficient of friction by ASTM D1894. The terminal product is a 20–23 µm machine-grade stretch film roll, typically 500 mm wide and 1,500 m long, for rotary pallet wrappers. Transverse chatter on the chill roll below 15°C is a production-scale failure linked to insufficient internal chill water flow; the corrective action is to raise roll temperature to 20°C and verify air knife volume before restarting.
Because 7120B is a 1-butene LLDPE with a 0.918 g/cm³ density and a 1.0 dg/min melt index, a 2.5:1 blow-up ratio on a high-stalk line collapses unless the compound is modified with 15–20 wt% LDPE. The LDPE fraction raises melt strength and stabilizes the bubble on an 80-mm extruder with a 30:1 L/D grooved-feed section, a 200-mm spiral mandrel die, and a 1.6-mm die gap. Frost line height is maintained at six to eight die diameters, and die melt temperature is held at 199–210°C. The formulation for a frozen-food packaging web uses 85 wt% 7120B, 15 wt% LDPE with a 2.0 dg/min melt index, erucamide slip at 600–1,000 ppm, and silica antiblock at 2,500–5,000 ppm. The blown film is converted into 40–50 µm pillow pouches for frozen vegetable and bakery overwrap. Direct food contact compliance is established under FDA 21 CFR 177.1520(c) for olefin polymers, subject to end-use extractive limitations for the finished film; under EU Regulation 10/2011 the overall migration limit is 10 mg/dm² in food simulant A, B, and D2 under the stated time and temperature conditions. Tensile properties are tested according to ASTM D882, Elmendorf tear according to ASTM D1922, and dart impact according to ASTM D1709. Organoleptic failure occurs when erucamide slip is overdosed above 1,500 ppm and migrates into the packaged food matrix; sensory transfer is evaluated by ASTM F1308 in end-use qualification. No amine-based antistat is added because the migration of low-molecular-weight amines can destabilize heat seal strength and produce off-taste.
| End Use | Regulation/Standard | Test Method/Designation | Critical Limit/Verification |
|---|---|---|---|
| Direct food-contact frozen food film | FDA 21 CFR 177.1520(c) | End-use extraction per paragraph (c) | Finished-film extractives within specified olefin limits |
| Direct food-contact frozen food film | EU Regulation 10/2011 | OM in simulant A, B, D2 | 10 mg/dm² |
| Heavy-duty industrial sacks | EU Packaging Directive 94/62/EC | EN 14582:2016 | Sum of Pb, Cd, Hg, Cr VI < 100 mg/kg |
| Pallet stretch wrap indirect food transport | FDA 21 CFR 177.1520 | End-use extraction | Olefin polymer specification met |
| Agricultural silage cover | REACH Annex XVII | ASTM G154 | Retained elongation after defined UV exposure |
Form-fill-seal conversion of heavy-duty sacks places a simultaneous demand on heat seal initiation temperature and hot-tack window; both parameters are measured per ASTM F88 and ASTM F1921. 7120B is employed in a three-layer blown film structure at 80 wt% in the core and sealant layers, with 20 wt% LDPE for melt strength and a 5 wt% HDPE fraction in the outer layer to increase stiffness and blocking resistance; the combined film caliper is 90 µm with a gusseted tube width of 360 mm. On a 90-mm extruder with a barrier screw and a 350-mm die gap of 2.2 mm, the blow-up ratio is 2.2:1 and the melt temperature is 215–230°C. The finished sack is used for chemical resin export, construction aggregate, and polymer powder packaging; it must pass a 1.2-m dart impact test according to ASTM D1709 and an Elmendorf tear test according to ASTM D1922, with minimum values specified by the end user, not by resin lot. Batch-to-batch variance in reground edge trim above 20 wt% produces gel accumulations in the 90-mm screw channels and causes seal interruption at 1.5 seals per minute on a commercial FFS line; this is controlled by keeping regrind below 20 wt% and by using a 100-mesh breaker plate. Heavy metal compliance for the ink-free sack structure follows EU Packaging Directive 94/62/EC, with the sum of lead, cadmium, mercury, and hexavalent chromium below 100 mg/kg when tested by EN 14582:2016.
Agricultural silage covers produced from 7120B-based blown film use either a 150-µm black monolayer or a 75-µm black/white coextrusion, the white layer containing 8–10 wt% titanium dioxide masterbatch for solar reflectance and the black layer 6–8 wt% carbon black masterbatch. A large-blown film conversion on a 90-mm extruder with a 500-mm die, 2.4-mm die gap, and 2.0:1 blow-up ratio is typical; melt temperature is 210–225°C to avoid degradation of the light stabilizer package. The compound is prepared with 0.3–0.5 wt% HALS and 0.2 wt% phenolic antioxidant; no low-molecular-weight amine antistat is used because it may bloom to the surface and accelerate carbon black rub-out. The terminal product is a 4-m-wide silage cover, 150 µm thick, used for bunker silo or bale wrap. UV resistance is evaluated by ASTM G154, with a criterion of less than 50% retained tensile elongation after 1,500 hours for seasonal covers. Long-term storage in contact with silage leachate below pH 4 requires verification of additive migration under REACH and national fertilizer-contact regulations; no direct food contact status is claimed.
Below haul-off speeds of roughly 180 m/min, the cast film edge bead is ordinarily manageable in 7120B sealant webs, but above 300 m/min the edge pinning force and draw resonance must be controlled by an air knife and by die-lip temperature profiling. Cast lamination structures for non-retort flexible packaging use 7120B as a 20–30 µm sealant layer on aluminium foil or PET, blended with 15–20 wt% LDPE to reduce neck-in. The web is coextruded with an ethylene acrylic acid copolymer tie layer when foil adhesion is critical; the tie layer comprises approximately 10% of total web thickness. Extrusion melt temperature is 280–300°C, die gap is 0.7 mm, and the substrate is primed with an ozone dose of 10–20 mg/m² or corona treatment to 42 dyne/cm. The composite is tested for seal strength per ASTM F88 and oxygen permeability per ASTM F1927. End products include dry beverage premix pouches and wet-wipe lidding, where the sealant must withstand a 25-second dwell at 150°C but is not intended for retort exposure above 121°C because the butene backbone lacks sufficient high-temperature creep resistance. When line speed is pushed to 350 m/min, the die exit film temperature measured by infrared pyrometer should not exceed 310°C; prolonged excursions above that value accelerate antioxidant consumption and create oxidation islands visible as yellow streaks. Published data for film performance above 400 m/min with this specific butene grade is limited; converter trials with a 0.55-mm die gap and a dual-zone chill roll are required before release.
A treated 18-µm overwrap web produced from 7120B on an 80-mm extruder benefits from the 1.0-dg/min melt index because the film can be drawn to a 2.0-mm die gap without excessive melt fracture. The application targets outer-wrap packaging for paper towel bundles and tissue multipacks, where the film is printed in flexo and surface-treated to 38–42 dyne/cm before printing. Formulation consists of 90 wt% 7120B and 10 wt% LDPE, with slip at 800–1,200 ppm and antiblock at 2,000–3,000 ppm. On a 220-mm die, the blow-up ratio is 2.0:1, frost line height is set at 500–700 mm, and die melt temperature is 200–215°C. The finished web is tested for dart impact by ASTM D1709, Elmendorf tear by ASTM D1922, and haze by ASTM D1003. Potential blocking in the roll is controlled by storage below 35°C and by avoiding winding tension above 12 N/cm. No direct food contact claim is made for the overwrap unless the converter validates the printed film under 21 CFR 177.1520 and the applicable food additive clearances for the printing ink and varnish.
Competitive Chevron Phillips Marlex® 7120B LLDPE Blown & Cast Film Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chevron Phillips Marlex® 7120B is a linear low-density polyethylene film resin produced with butene as the short-chain branching comonomer. The nominal melt mass-flow rate is 1.0 g/10 min measured at 190 °C under a 2.16 kg load according to ASTM D1238 or ISO 1133-1:2022, and the nominal density is 0.918 g/cm³ according to ASTM D1505 or ISO 1183-1:2019. The material is supplied as pellets and is intended for blown film and cast film extrusion. The combination of melt index and density places the resin in the Ziegler-Natta butene LLDPE class, in which film toughness and heat-seal response depend more on short-chain branch distribution and extrusion orientation than on molecular weight alone. The resin is not a high-pressure LDPE; the linear backbone produces lower melt tension and different neck-in behavior in cast film.
| Property | Test standard | Typical value | Unit |
|---|---|---|---|
| Melt mass-flow rate | ASTM D1238 / ISO 1133-1:2022 | 1.0 | g/10 min |
| Density | ASTM D1505 / ISO 1183-1:2019 | 0.918 | g/cm³ |
| Comonomer type | Supplier FTIR | Butene | — |
| Process applicability | — | Blown film, cast film | — |
Because the comonomer is butene, the short-chain branch length is shorter than that of a hexene copolymer but longer than that of an ethylene homopolymer. The crystallization rate is moderate, allowing post-bubble quenching to control film density and shrinkage. On blown film lines, high cooling-air rates and low frost line settings freeze the film before the broad low-molecular-weight fraction can develop large spherulites; this improves clarity but can reduce transverse-direction tear. On cast film lines, the higher cooling rate at the chill roll produces a film with lower crystallinity and higher dart impact than slow cooling; this behavior is generic to LLDPE and should be verified by differential scanning calorimetry per ASTM D3418 and tensile testing per ASTM D882.
| Process | Parameter | Start-up range |
|---|---|---|
| Blown film | Melt temperature | 180 °C to 205 °C |
| Blown film | Die gap | 1.5 mm to 2.5 mm |
| Blown film | Blow-up ratio | 2.0:1 to 2.8:1 |
| Cast film | Die exit melt temperature | 220 °C to 240 °C |
| Cast film | Die gap | 0.5 mm to 1.0 mm |
| Cast film | Air gap | 15 mm to 30 mm |
For blown film extrusion, a melt temperature of 180 °C to 205 °C and a die gap of 1.5 mm to 2.5 mm are common start-up conditions. Because the melt index is 1.0 g/10 min, the resin has lower melt strength than a 0.5 MI fractional-melt LLDPE; lower-stalk bubble geometry is preferred, and frost line heights above 8 die diameters may produce bubble oscillation on single-lip air-ring systems. A blow-up ratio between 2.0:1 and 2.8:1 is typical for balanced machine-direction and transverse-direction tensile properties. If haze must be reduced, lowering melt temperature by 5 °C to 10 °C within this range and increasing die gap to 2.0 mm or larger generally improves surface uniformity, but the change also reduces melt strength at the bubble neck.
In cast film, die exit melt temperature is normally set between 220 °C and 240 °C. The die gap may range from 0.5 mm to 1.0 mm, and air gap is controlled between 15 mm and 30 mm. Neck-in and edge bead must be measured against the incumbent resin at the same melt temperature and line speed. At this density, the melt curtain has lower extensional viscosity than high-molecular-weight LLDPE, so draw resonance can occur when line speed increases without increasing die temperature or reducing air gap. Operators should record melt curtain position and thickness across the web every 30 min during the first trial, because the resin’s neck-in behavior is line-specific and published data for this specific configuration is limited.
The 1.0 melt index does not by itself define lot-to-lot variation. A melt flow rate ratio, if supplied, can indicate the breadth of molecular weight distribution. For Ziegler-Natta butene LLDPE, broader distribution can improve processability but may increase gel formation when the resin is overheated. Gel count is not a general resin specification; if gels are visible, the extrusion system should be inspected first for dead spots in the screen pack, adapter, or die lips. On a 65 mm grooved-feed extruder with 24:1 L/D, gel generation is commonly associated with localized temperatures above 230 °C at the screw tip rather than with pellet contamination. This processing boundary applies to many LLDPE grades and is not unique to 7120B.
Typical uses are industrial liners, stretch wrap core layers, carrier films, and overwrap structures in which dart impact, tear resistance, and thickness control are specified. In coextruded cast stretch film, 7120B is placed in a core layer between metallocene LLDPE cling and release layers; the core contributes stiffness and puncture resistance while the skins control cling. In blown film liners, the resin is run in monolayer and coextruded structures from 20 µm to 150 µm. Mechanical acceptance should be measured according to ASTM D882 for tensile properties, ASTM D1709 for dart drop, and ASTM D1922 for Elmendorf tear. Because these values are thickness-dependent and sensitive to blow-up ratio and cooling rate, a target-line trial is required for specification setting.
Compared with a 0.5 MI fractional-melt LLDPE of similar density, 7120B generates lower melt pressure and lower screw torque at the same output. The penalty occurs in bubble stability: the lower melt strength widens the bubble neck and makes the film more sensitive to frost line height and air-ring flow. In cast film, the higher MI reduces edge bead and permits faster line startup, but critical draw ratio is lower than for a fractional-melt grade. Heat-seal initiation for a 0.918 g/cm³ butene LLDPE typically lies between 100 °C and 115 °C, but users should compare hot tack according to ASTM F1921 because seal strength alone does not predict high-speed packaging performance.
Against a hexene LLDPE of the same density and melt index, the butene branch in 7120B is shorter and generally less efficient at forming tie molecules between lamellae. Dart impact per ASTM D1709 and Elmendorf tear per ASTM D1922 are therefore typically lower in a butene resin at equal gauge. The degree of difference depends on coextrusion layer ratio, die gap, and frost line height, and published data for this specific 7120B-to-hexene comparison is limited. Against high-pressure LDPE, the linear backbone of 7120B reduces shear-thinning and long-chain branching; extrusion may require a narrower die gap or higher melt temperature to control thickness uniformity, while tensile strength at break measured per ASTM D882 is generally higher at the same gauge. Against metallocene LLDPE, the broader molecular weight distribution of a Ziegler-Natta butene resin can reduce die-lip buildup on long cast film campaigns, but it typically yields lower gloss and higher haze. Haze values below 5% are more characteristic of metallocene LLDPE at 25 µm, while butene LLDPE grades of this density often fall in the 8% to 15% range under ASTM D1003; the final value depends on cooling air and die-lip finish.
Substitution on existing blown film lines should begin with a trial at the incumbent conditions, then adjust only one variable at a time. If an LDPE bubble is being replaced, reduce the blow-up ratio by 0.5 units and lower the frost line height before increasing throughput. If a hexene LLDPE is being replaced, monitor dart impact and Elmendorf tear on film sampled at the same gauge and the same blow-up ratio. On cast film lines, measure neck-in as a percentage of die width within the first 20 min of stable running; a change greater than 2% from the incumbent is an indication to adjust melt temperature or die gap. For coextruded structures, the resin should not be placed in a skin layer if low seal initiation temperature or high clarity is required; a metallocene LLDPE skin is preferred in those applications.
Food-contact status must be confirmed with the supplier’s compliance certificate. Polyethylene film resins of this composition are generally used under FDA 21 CFR 177.1520 and European Union Regulation (EU) No 10/2011 when authorized additives and processing conditions are applied. The polymer itself is exempt from registration under REACH Article 2(9), but monomer and additive registrations must be maintained by the supplier. RoHS Directive 2011/65/EU restrictions on lead, mercury, cadmium, hexavalent chromium, PBB, and PBDE do not apply to the neat polyolefin resin unless contaminated by external processing equipment. No pre-drying is required at storage relative humidity below 60%; if pellet surface condensation occurs from temperature cycling, purge with dry resin and avoid drying above 60 °C because pellet agglomeration may form. Avoid blending with amine-based antifog or slip concentrates beyond supplier-approved ratios, because migration products can accumulate on the die lip at cast film melt temperatures and create edge tear. The resin should not remain at melt temperature above 200 °C for extended line stops longer than 30 min; purging with a lower-viscosity polyolefin is preferred during shutdown.