    Specifications
    HS Code 222601
    Density 0.918 g/cm³
    Melt Index 190 C 2 16 Kg 1.0 g/10 min
    Comonomer Butene-1
    Melting Point Dsc 122 °C
    Vicat Softening Point 101 °C
    Tensile Strength At Yield Md 10.3 MPa
    Tensile Strength At Break Md 30.0 MPa
    Tensile Strength At Break Td 27.6 MPa
    Elongation At Break Md 700%
    Elongation At Break Td 800%
    Dart Drop Impact 120 g
    Elmendorf Tear Strength Md 250 g/mil
    Elmendorf Tear Strength Td 400 g/mil
    Haze 10%
    Gloss 45 60%
    Coefficient Of Friction 0.2

    As an accredited Chevron Phillips Marlex® 7109DJ LLDPE Blown Film Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Chevron Phillips Marlex® 7109DJ LLDPE Blown Film Resin is supplied in 25 kg polyethylene-lined multiwall bags, palletized for handling.
    Container Loading (20′ FCL) 20′ FCL: Marlex 7109DJ LLDPE in 25 kg bags on pallets, about 18–20 MT net, securely loaded and braced.
    Shipping Chevron Phillips Marlex® 7109DJ LLDPE Blown Film Resin is shipped as non-hazardous resin pellets, typically in 25 kg polyethylene bags or bulk containers, palletized and stretch-wrapped. Transport in dry, clean vehicles, avoiding heat, sunlight, and ignition sources. Not DOT/IMDG/IATA regulated. Store under cover in a dry, ventilated area.
    Storage Store Marlex® 7109DJ LLDPE resin in a cool, dry, clean, well-ventilated area away from direct sunlight, heat, ignition sources, moisture, and strong oxidizers. Keep original bags or containers closed and off the floor to prevent contamination. Avoid excessive stacking and temperatures that could soften or degrade pellets. Use first-in, first-out rotation and follow the SDS/local regulations.
    Shelf Life Typically 12 months when stored in original packaging in a cool, dry, ventilated area away from heat and direct sunlight.
    Application of Chevron Phillips Marlex® 7109DJ LLDPE Blown Film Resin

    Outdoor Exposure Mechanics in Silage Bale Wrap and Agricultural Stretch Film

    Chevron Phillips Marlex® 7109DJ LLDPE blown film resin, specified with nominal density 0.918 g/cm³ (ASTM D1505) and melt index 1.0 g/10 min (ASTM D1238, 190°C/2.16 kg), is processed for silage bale wrap as a three-layer coextruded film. The core layer carries 60 wt%–80 wt% of the resin, with 15 wt%–25 wt% lower-melt-index hexene LLDPE or metallocene LLDPE to raise dart impact and low-temperature puncture resistance, 3 wt%–5 wt% white UV-reflective masterbatch, 1.0 wt%–1.5 wt% HALS-based UV stabilizer masterbatch, and 0.5 wt%–1.0 wt% cling additive in the outer skin. Regulatory compliance for agricultural silage film is referenced against EN 13207:2018 for silage barrier and mechanical requirements; tensile properties after weathering are measured under ASTM D882-18, and edge tear is measured under ASTM D1922-15. Carbonate-filled formulations are excluded because they reduce tear resistance below the 400 g/25 µm threshold commonly required for wrapped grass silage.

    Production-scale conversions observed on a 75 mm grooved-feed extruder with 30:1 L/D barrier screw use a 250 mm three-layer annular die with 2.0 mm die gap, 2.5:1–3.0:1 blow-up ratio, and frost line height 8–10 die diameters. Melt temperature at the die is held at 200°C–215°C, with output 250 kg/h–350 kg/h and internal bubble cooling engaged to maintain thickness variation below ±4%. Winding is configured with taper tension 0.5 N/mm–1.0 N/mm to prevent edge wrinkles at 750 mm × 1500 m finished rolls. Terminal finished products are silage bale wrap, haylage wrap, and maize silage wrap, applied on balers at 55%–70% pre-stretch. The resin itself does not provide UV stabilization; storage exposure beyond 12 months requires increased HALS concentration or secondary sleeve protection.

    In frozen-food packaging lines operating at 25 µm–60 µm sealant-gauge targets, 7109DJ is blended at 80 wt% with 15 wt% high-pressure LDPE and 5 wt% synthetic silica antiblock masterbatch for monolayer printed bags, or used as the sealant layer at 20 wt%–25 wt% of total structure in a coextruded construction with EVOH or polyamide core. Food-contact compliance rests on FDA 21 CFR 177.1520(c) 3.2a and 3.2b for olefin polymers, EU Regulation (EU) No 10/2011 Annex I with overall migration limit 10 mg/dm², and China GB 4806.7-2016 for food-contact plastic articles. The blown film process uses a 45 mm–65 mm extruder with 24:1–30:1 L/D barrier screw, die gap 1.8 mm–2.2 mm, blow-up ratio 2.0–2.3, and melt temperature 190°C–210°C.

    On high-speed vertical form-fill-seal lines at 45 m/min–80 m/min, seal bar temperature is maintained at 115°C–135°C with dwell 40 ms–80 ms and sealing pressure 0.3 MPa–0.6 MPa. Terminal types include frozen vegetable pillow bags, IQF fruit pouches, frozen seafood bags, and ice-cream overwrap. Seal strength under ASTM F88/F88M-21 typically exceeds 12 N/25 mm for 50 µm film at 125°C seal-bar temperature. The operational boundary is that antiblock loading above 8 wt% raises seal initiation temperature by approximately +5°C and reduces dart impact, so the combined additive masterbatch should remain below 6 wt%.

    What Differs in High-Dart Heavy-Duty Sack Film Compared with General-Purpose Liner Applications?

    Heavy-duty sack lines operate with film gauges from 70 µm to 150 µm and target high dart impact, tear propagation resistance, and low water vapour transmission for hygroscopic polymer shipments. A typical formulation uses 70 wt%–85 wt% 7109DJ, 15 wt%–30 wt% LDPE to enhance bubble stability, and for outdoor storage specification, 1.0 wt%–2.0 wt% carbon black masterbatch with 0.2 wt%–0.5 wt% polymer processing aid to suppress melt fracture at high throughput. Compliance is anchored to ASTM D1709-16a for dart impact, ASTM D1922-15 for Elmendorf tear, ASTM D882-18 for tensile properties, and ASTM D2103 for polyethylene film dimensional tolerance; FIBC liner insertion uses gusseted tube dimensions consistent with ISO 21898:2004 packaging requirements.

    A 300 mm–600 mm annular die with 2.0 mm–2.5 mm die gap, 2.0:1–3.0:1 blow-up ratio, internal bubble cooling, and 8 m–12 m frost line height yields gauge variation below ±5%. Melt temperature at the die is 195°C–220°C. On a 90 mm grooved-feed extruder with 30:1 L/D screw, screw speed is limited so that post-screen pressure remains below 450 bar. Terminal products include polymer pellet shipping sacks, mineral and cement liners, fine chemical bulk liners, and FIBC liners. Field failure mode is bubble side-wall instability when blow-up ratio exceeds 3.0:1 without internal bubble cooling; the resulting gauge bands reduce dart impact by more than 20% relative to stable gauge film.

    Lamination sealant webs for stand-up pouches and bag-in-box liners impose a narrow heat-seal initiation window because downstream packaging speeds exceed 60 m/min. The sealant layer is formulated at 70 wt% 7109DJ with 30 wt% lower-density LDPE or metallocene LLDPE, and 1 wt%–2 wt% slip/antiblock masterbatch. It is converted into 15 µm–30 µm blown film and adhesive-laminated to PET or oriented nylon; total laminate thickness ranges from 70 µm to 120 µm. Food-contact compliance follows FDA 21 CFR 177.1520(c) 3.2b, EU Regulation (EU) No 10/2011 including specific migration provisions for multilayer laminates, and GB 9685-2016 for additives in food-contact polymers. Non-food bag-in-box uses, such as liquid detergent liners, are assessed under REACH 1907/2006 Annex XVII restrictions for phthalates and heavy metals.

    The blown sealant film is produced with a 60 mm extruder, 28:1 L/D barrier screw, 2.0 mm die gap, 2.2:1 blow-up ratio, and melt temperature 195°C–205°C. Surface treatment by corona discharge is set to 38 mN/m–42 mN/m; below 38 mN/m, lamination bond strength measured under ASTM F904 may fall below 2.5 N/15 mm. Terminal products include stand-up pouches for tomato paste, bag-in-box liners for cold-chain dairy, wine bag-in-box sealant plies, and liquid detergent refill pouches. The operational boundary is that continuous service temperature above 70°C or retort sterilization at 121°C exceeds the softening range of this resin.

    When Blown Film Replaces Cast Extrusion for Hand-Applied Pallet Wrap

    Hand-applied pallet wrap produced from blown tube uses a formulation of 90 wt% 7109DJ, 8 wt% metallocene LLDPE, and 2 wt% cling additive masterbatch, at thickness 12 µm–20 µm. Performance data are reported under ASTM D882-18 for tensile properties and ASTM D1894-14 for coefficient of friction; cling is evaluated by unwind force and peel adhesion methods specific to stretch-film converters. The blown process uses a 200 mm–350 mm annular die, 2.0 mm die gap, 2.0:1–2.8:1 blow-up ratio, melt temperature 190°C–210°C, and output per die circumference 0.8 kg/h/mm–1.5 kg/h/mm.

    On pallet wrapping machines, elongation is limited to 100%–200% for hand wrapping; blown film typically retains higher machine-direction tensile strength but lower ultimate stretch than cast film. Terminal products are hand wrapper rolls at 450 mm × 300 m–600 m for appliance bundling, furniture protection, and mixed-pallet shipment. The limitation is that power pre-stretch above 250% is not recommended because neck-in and inconsistent cling may occur; published data for this specific configuration is limited, and cast-grade LLDPE remains the standard for high-speed machine pallet wrap.

    Construction Vapour Retarder and Temporary Containment Film Property Requirements

    Under-slab vapour retarder and temporary containment film use 7109DJ at 85 wt% with 15 wt% LDPE and 2 wt% carbon black masterbatch for UV-stabilized black sheeting; film thickness ranges 100 µm–250 µm. Compliance is governed by ASTM E1745 for flexible water vapour retarders, ASTM E96/E96M-21 for water vapour transmission, ASTM D4397 for polyethylene sheeting in construction, and ASTM D1709-16a for puncture impact. The resin provides the base polymer for a Class A vapour retarder only when thickness and lamination are specified appropriately; the actual permeance must be verified under ASTM E96/E96M-21 desiccant method.

    Standard designationTechnical requirementApplication-specific acceptance basis
    ASTM E96/E96M-21Water vapour transmission rate desiccant methodPermeance reported at specified thickness; no pass without measured value
    ASTM E1745Flexible water vapour retarder specificationClass A, B, or C assignment by permeance and thickness
    ASTM D1709-16aDart impact method ATypical acceptance 500 g for 150 µm under-slab film
    ASTM D4397Polyethylene sheeting for constructionWidth/length tolerance ±2%

    Blown-film conversion for this gauge employs a 400 mm die, 2.5 mm die gap, 2.5:1–3.5:1 blow-up ratio, internal bubble cooling with thickness control ±5%, and melt temperature 200°C–225°C. Gusseted film is folded to 3 m–6 m layflat widths for slab placement. Terminal products include under-slab vapour barriers, wall vapour retarder membranes, dust containment sheeting, lead abatement barriers, and temporary weather protection films. The operational boundary is that contact with bitumen or solvent-based adhesives may plasticize the film; compatibility must be tested before specification.

    Free Quote

    Competitive Chevron Phillips Marlex® 7109DJ LLDPE Blown Film Resin prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Chevron Phillips Marlex® 7109DJ is a linear low density polyethylene blown film resin polymerized with 1-hexene as the short-chain branching comonomer. The nominal density is 0.918 g/cm3, and the nominal melt flow rate is 1.0 g/10 min when determined at 190 °C under a 2.16 kg load in accordance with ASTM D1238. Because the melt flow rate places the material between fractional-melt film grades and high-output casting grades, the resin is typically selected for general-purpose blown film lines where bubble stability and dart impact are balanced against extrusion pressure. The pellet form and antioxidant package are designed for conventional single-screw extrusion, but published data for lot-to-lot variability on specific barrier-screw configurations is limited; converters should verify each lot against the certificate of analysis before entering production.

    Specification Profile and Test Designations

    Resin-level values for 7109DJ are reported under standardized conditions. The density method in ASTM D1505 uses a gradient column equilibrated at 23 °C. A shift of 0.001 g/cm3 is meaningful for LLDPE film performance: moving from 0.918 g/cm3 to 0.920 g/cm3 can increase stiffness but reduce dart impact. Because density and comonomer content are correlated, the resin should be sampled at regular intervals and tested with the same density column to track lot-to-lot drift. The melt flow rate test is a single-point test and does not represent the full viscosity curve.

    PropertyNominal ValueTest Designation
    Density0.918 g/cm3ASTM D1505
    Melt Flow Rate (190 °C, 2.16 kg)1.0 g/10 minASTM D1238
    DSC melting peakapproximately 122 °CASTM D3418

    Film-level properties such as dart impact, Elmendorf tear, tensile strength, and haze are generated on fabricated film, not on pellets. For a 25 µm film produced at 2.5:1 blow-up ratio, the values reported in published technical data depend on the specific extrusion line, die gap, frost line height, and cooling air temperature. Therefore, the values should be treated as comparative references rather than guaranteed product specifications. The converter should generate its own data using the target line and the following methods: ASTM D1709 for dart impact, ASTM D1922 for Elmendorf tear, ASTM D882 for tensile properties, and ASTM D1003 for haze.

    Under production-scale conditions on a 45 mm single-screw extruder with 30:1 L/D and a barrier-flight screw with a Maddock mixing section, melt temperatures of 190 °C to 230 °C are commonly used for 7109DJ. On a 60 mm extruder with 28:1 L/D, barrel set-points are often set with the feed throat at 40 °C to 50 °C, the compression zone at 180 °C to 200 °C, and the metering zone at 200 °C to 220 °C. These profiles are specific to smooth-bore feed sections; grooved-feed extruders may require a different rear-zone temperature to avoid melting in the feed section. If melting occurs in a grooved-feed section, torque rises and feed instability may appear as screw-speed-dependent output fluctuations. The shear viscosity at extrusion shear rates is not captured by the melt flow test; capillary rheometry at 190 °C and shear rates from 100 s-1 to 1000 s-1 is required for screw design and pressure-drop calculations. At lower melt temperatures, melt pressure can exceed the manufacturer’s limit for melt pumps and screen changers. At upper temperatures, oxidative gel formation may occur. Oxidized gel defects in LLDPE film can be quantified by counting visible gels per square meter under a calibrated light table, although published data for this specific resin is limited.

    What Process Parameters Govern Bubble Stability and Gauge Uniformity?

    Bubble stability in hexene-copolymer LLDPE is governed by die gap, blow-up ratio, frost line height, and air-ring cooling. Machinery manufacturer guidelines for fractional-melt LLDPE indicate die gaps from 1.5 mm to 2.5 mm and blow-up ratios from 2.0:1 to 3.0:1. A narrow die gap increases shear stress and can improve gauge uniformity but may initiate sharkskin melt fracture at high output rates when the melt temperature is below 190 °C. Frost line height should be high enough to allow adequate crystallization before bubble collapse; if the frost line is set too low, film blocking and gauge bands can occur. The air ring should be adjusted to produce a stable neck. High-stalk bubbles are generally not preferred for this density unless the extruder is equipped with internal bubble cooling. On lines without internal bubble cooling, the maximum output may be limited by bubble breathing rather than by the screw melting capacity.

    Die diameters above 200 mm create gauge uniformity challenges because melt temperature distribution across the die governs local viscosity. Use of dual-lip air rings and internal bubble cooling is common on high-output LLDPE lines. A spiral mandrel die with a die gap of 1.8 mm to 2.2 mm is typical, but interchange between spiral and crosshead dies requires re-optimization. Because shear heating depends on screw speed, melt temperature should be measured by an immersion probe at the adapter rather than by barrel set-points. Pressure transducers at the screen changer and die inlet provide early warning of gel accumulation; a rise in differential pressure greater than 20% over the baseline at constant screw speed may indicate screen blockage or resin degradation, but individual line limits set by the equipment manufacturer supersede this value.

    When Hexene Comonomer Replaces Butene in Blown Film Structures

    Relative to a butene-copolymer LLDPE of equivalent 0.918 g/cm3 density and 1.0 g/10 min melt flow rate, the 1-hexene comonomer in 7109DJ increases the length of short-chain branches and can improve tie-molecule formation between lamellae. The resulting film typically shows higher dart impact strength when tested under ASTM D1709 and higher Elmendorf tear resistance when tested under ASTM D1922, while maintaining a comparable secant modulus. However, the improvement is not uniform across all draw ratios; at high stalk heights and high machine-direction orientation, the tear balance can shift, and published data for this specific configuration is limited.

    Compared with autoclave LDPE, 7109DJ exhibits a linear backbone without long-chain branching, so melt strength is inherently lower. This behavior is observable as lower bubble stability at low output rates and can be quantified by melt strength tests such as capillary breakup methods, though published data for this specific resin is limited. Therefore, LDPE is often added at 10–30 wt% to improve bubble stability and optical properties. The addition changes the film’s tensile and dart response; the converter must re-establish the film data using ASTM D882 for tensile and ASTM D1709 for dart impact. Unlike metallocene-catalyzed LLDPE, the optical clarity of 7109DJ may be lower because the molecular weight distribution is broader; haze measurements under ASTM D1003 should be specified before high-clarity applications are considered.

    In comparison with octene-copolymer LLDPE of similar density and melt flow rate, the hexene-copolymer resin may show lower dart impact in some high-toughness constructions, but processing window and melt pressure behavior are often more favorable on standard blown film lines. Published comparative data for this specific resin under identical film conditions is limited; converter trials should be designed with a fixed die gap, blow-up ratio, and frost line height to isolate resin effects.

    On multi-layer blown film lines, 7109DJ can occupy core or skin layers depending on sealant requirements. In a three-layer A/B/C structure, using 7109DJ in the core layer with a lower-melt-index metallocene in the skin can improve dart impact while retaining low-temperature seal initiation. The seal initiation temperature should be determined using ASTM F88 across a range of sealing temperatures rather than by a single fixed setting. Compared with ionomer sealants, the LLDPE seal strength is lower at comparable seal bar settings, and the hot-tack window is narrower; converters must validate hot-tack using ASTM F1921 if form-fill-seal operations are planned.

    Dart Impact and Elmendorf Tear as Nonlinear Functions of Draw Ratio

    Film data for LLDPE are not scalable from a single point. At 25 µm thickness and 2.5:1 blow-up ratio, dart impact measured under ASTM D1709 may reflect isotropic orientation. As thickness increases to 50 µm, elongation at break and tear resistance often increase, but dart impact response can become dominated by yield-stress propagation rather than film stretching. At blow-up ratios below 2.0:1, machine-direction orientation increases, and Elmendorf tear in the transverse direction can decline sharply. At blow-up ratios above 3.0:1, transverse orientation dominates, and machine-direction tear may fall. These property shifts are the result of anisotropic crystalline orientation and cannot be predicted from resin density or melt flow alone. A statistically designed trial with thickness, blow-up ratio, frost line height, and die gap as variables is required. The data should be analyzed using ASTM D1709, ASTM D1922, and ASTM D882; the number of replicates should follow the precision statements in each method.

    Because 7109DJ is a hexene-copolymer LLDPE, the dart impact improvement over butene-copolymer LLDPE is often most visible at 25 µm to 50 µm thickness. At thickness below 20 µm, film gauge variation can exceed 10% unless the line is equipped with automatic profile control, and this variation can mask differences between comonomer types. For thin-gauge applications, online capacitance gauges with feedback to the air ring should be used to hold thickness variation within ±5% before comparative property tests are accepted.

    Post-industrial reclaimed LLDPE can be added at 20–40 wt% if the reclaimed stream is clean and free of polypropylene or HDPE contamination. Contamination with 5 wt% polypropylene can create haze bands and unpelletized gels. The melt flow rate of recycled material should be within ±0.3 g/10 min of the virgin resin to avoid gauge variability. If the reclaimed stream contains printing inks or tie resins, barrier-layer adhesion must be retested according to ASTM F904 for lamination bond strength.

    Regulatory Boundary Conditions for Fatty-Food Packaging Films

    Compliance statements for olefin polymers used in food contact are contingent on the finished article’s thickness, temperature, and food-simulant classification. In the United States, unmodified polyethylene intended for food contact may be subject to 21 CFR 177.1520(c), with paragraph classifications depending on density and extraction behavior. Converters should not assume that pellet compliance alone covers the finished film; residual processing aids, inks, and adhesives can require separate migration review. Under EU Regulation 10/2011, overall migration into food simulants must be tested according to the applicable simulant, time, and temperature conditions specified in the regulation, and the specific migration of authorized additives must be confirmed by analytical testing.

    For fatty foods, the use of food simulant D2 or 95% ethanol under the prescribed time–temperature conditions is common, but selection depends on the food contact category. Published data for this specific resin under all EU food-simulant categories is limited; therefore, qualification should be performed on the final production film. The resin is not intended for retort or hot-fill packaging above 90 °C because the softening behavior of LLDPE reduces dimensional stability.

    At melt temperatures above 250 °C, LLDPE undergoes oxidative degradation that can form crosslinked gels and shift the melt flow rate. If a converter observes an increase in melt flow rate after prolonged residence time, the cause is usually chain scission from oxidation; if the melt flow rate decreases, crosslinking may dominate. The barrel residence time should be kept below 15 min at full production rate, and start-up purges should use a lower-melt-index polyethylene to remove degraded material from dead spots. These limits are general for LLDPE; published data for 7109DJ under extended purge conditions is limited.