| HS Code | 533121 |
| Productname | Chevron Phillips Marlex® 7104 LLDPE Sheet Extrusion |
| Manufacturer | Chevron Phillips Chemical Company |
| Polymertype | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene-1 |
| Processingmethod | Sheet Extrusion |
| Density | 0.918 g/cm³ |
| Meltindex | 0.8 g/10 min (190°C/2.16 kg) |
| Tensilestrengthatyield | 10.3 MPa (1500 psi) |
| Tensilestrengthatbreak | 20.7 MPa (3000 psi) |
| Elongationatbreak | 800% |
| Flexuralmodulus | 207 MPa (30,000 psi) |
| Vicatsofteningpoint | 100°C |
| Meltingpoint | 123°C |
| Brittlenesstemperature | Below -70°C |
| Hardnessshored | 50 |
| Environmentalstresscrackresistance | Greater than 1000 hours |
| Thermalexpansioncoefficient | 1.5E-4 cm/cm/°C |
| Waterabsorption | Less than 0.01% |
As an accredited Chevron Phillips Marlex® 7104 LLDPE Sheet Extrusion factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Chevron Phillips Marlex® 7104 LLDPE Sheet Extrusion is packaged in 25 kg bags, with 40 bags per 1,000 kg pallet. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with palletized 25 kg bags of Chevron Phillips Marlex® 7104 LLDPE for sheet extrusion, securely strapped. |
| Shipping | Chevron Phillips Marlex® 7104 LLDPE Sheet Extrusion resin ships as non-hazardous, free-flowing pellets, typically in 25 kg moisture-barrier bags, palletized and stretch-wrapped. Transport in clean, dry trucks or containers. Protect from heat, sunlight, moisture, and contamination. Store cool, dry, and use first-in, first-out. Handle carefully to prevent package damage. |
| Storage | Store in original, unopened packaging in a cool, dry, well-ventilated warehouse. Keep away from direct sunlight, heat, flames, ignition sources, and incompatible materials. Palletize off the floor, avoid excessive stacking, and protect from moisture, dust, odors, and UV exposure. Keep containers sealed and labeled. Follow first-in, first-out stock rotation and consult the SDS for local requirements. |
| Shelf Life | Store in a cool, dry, ventilated area away from direct sunlight and moisture; shelf life is indefinite when properly stored. |
Marlex® 7104 LLDPE is specified for flat-die sheet extrusion lines in which low-temperature puncture resistance, weldability, and melt stability operate as co-dependent variables. On sheet lines from 1.2 m to 3.0 m die width, the melt temperature band is maintained at 210°C–240°C; chill-roll temperatures below 55°C produce surface haze, and temperatures above 85°C increase roll-face blocking. The downstream scenarios below are separated by formulation objective, conversion equipment, and end-use compliance boundary, not by generic polyethylene type.
Marlex® 7104 is loaded at 95.0–97.5 wt% in black geomembrane sheet, with carbon black masterbatch metered to hold final carbon black at 2.0–3.0 wt% as required by GRI-GM13 and the oxidative resistance clauses of ASTM D5397. On a 2.4 m coat-hanger die fed by a 30:1 L/D single-screw extruder, melt temperature at the die lip is kept at 210°C–240°C, and polished chill rolls are held between 65°C and 85°C; chill-roll temperature drift greater than ±3°C is associated with transverse gauge bands above 0.05 mm. The converter-side additive system meters antioxidant masterbatch at 0.10–0.30 wt%; hindered phenolic/phosphite architecture is used to maintain oxidative induction time above 100 min at 200°C under ASTM D3895. Mechanical certification for a 1.0 mm sheet normally references ASTM D638 tensile yield at or above 11 MPa, ASTM D1004 tear strength at or above 45 N for 0.75 mm sheet, ASTM D4833 puncture resistance at or above 240 N for 1.0 mm sheet, and ASTM D5397 notched constant tensile load of at least 400 h. Edge-trim regrind is limited to 20 wt% because each heat history lowers oxidative induction time by 15–25 min per pass; when regrind exceeds 20 wt%, the antioxidant masterbatch must be re-dosed upward and the batch re-qualified. Carbon black above 3.5 wt% reduces wedge-weld peel strength below 80 N/cm under ASTM D6392 because the viscosity rise slows interdiffusion across the weld plane. Terminal products include landfill base liners, landfill cap sheets, heap leach pads, evaporation pond liners, wastewater lagoon covers, and double-containment sump liners.
| Formulation or process deviation | Measurement anchor | Observed failure mode |
|---|---|---|
| Final carbon black below 2.0 wt% | ASTM D1603 | GRI-GM13 oxidative induction time falls below 100 min |
| Final carbon black above 3.5 wt% | ASTM D6392 | Wedge-weld peel strength drops below 80 N/cm |
| Regrind addition above 20 wt% | ASTM D3895 | OIT loss of 15–25 min per heat history |
| Chill-roll drift above ±3°C | Contact roll pyrometer | Transverse gauge band above 0.05 mm |
Food-contact sheet extrusion based on Marlex® 7104 typically blends the resin with 15–30 wt% LDPE or 5–15 wt% HDPE to improve thermoforming melt strength and die-cutting rigidity. The resin blend is metered with slip/antiblock masterbatch at 1.0–2.0 wt%, yielding final erucamide concentrations of 300–800 ppm and synthetic silica concentrations of 500–1200 ppm; these additives reduce film-to-film blocking during roll winding and assist vacuum-forming release. Compliance under FDA 21 CFR 177.1520(c) paragraphs 3.1a and 3.2a covers olefin polymers for direct food contact, while EU harmonized testing is performed according to Regulation (EU) No 10/2011 Annex III and Annex V with simulant D1 for fatty foods and simulant A for aqueous foods. On a flat-die sheet line with 0.25–0.80 mm die gap, melt temperatures are kept at 205°C–230°C, and the cast sheet exits into a three-roll stack with roll temperatures of 55°C–75°C to balance surface gloss against post-trim shrinkage. Downstream thermoforming uses plug-assisted pressure/vacuum stations at sheet surface temperatures between 115°C and 130°C; cycle times for shallow trays are 3–8 s, with plug speed limited below 250 mm/s because Marlex® 7104 begins to exhibit draw-induced thinning at higher plug displacement rates. Terminal products include low-temperature frozen food trays, ice cream cup lids, fresh produce punnets, and thin-walled dairy portion cups that require sub-zero impact toughness rather than hot-fill resistance. The operational boundary is fixed: continuous exposure above 65°C or hot-fill pasteurization above 75°C is outside the product envelope because the Vicat softening point of the sheet falls below the thermal load exerted by steam or immersion retort. Edge-trim regrind is constrained to 15 wt% in food-contact layers unless migration testing is repeated, because variability in contaminant carryover from post-industrial scrap can invalidate the compliance declaration.
The formulation for underslab barrier sheet is maintained at 96.0–98.0 wt% Marlex® 7104, 2.0–3.0 wt% carbon black masterbatch, and 0.10–0.20 wt% hindered phenolic/phosphite stabilizer masterbatch; the carbon black concentration is set not for UV resistance but for opacity and pinhole visibility during installation. Flat-die extrusion at 0.20–0.50 mm thickness uses melt temperatures of 210°C–240°C and chill rolls at 60°C–80°C, after which the web is slit to 2.4–6.0 m panels. Under ASTM E1745, Class A requires water vapor permeance no greater than 0.1 perm when tested by ASTM E96 desiccant method at 23°C and 50% RH; tensile strength and puncture resistance are measured by ASTM D882 and ASTM D1709 respectively, and the sheet must retain these values after conditioning. The use of post-consumer regrind is not automatically excluded but is limited to 10 wt%; at higher addition, the melt flow index drift across the die can exceed 0.15 g/10 min, creating microtears that raise water vapor transmission above the 0.1 perm limit. Terminal products are underslab vapor retarders, radon barriers, crawl space liners, foundation protection layers, and below-grade waterproofing membranes. The product is not designed for direct UV exposure beyond 30 days unless a separate UV-stabilized cap layer is added to the sheet structure.
Within agricultural sheet conversion, black/white coextrusion positions Marlex® 7104 in the black core and black skin layers, where the resin is diluted to 96.0–97.0 wt% with a carbon black masterbatch targeting 2.0–3.0 wt% carbon black. The white layer is a separate LLDPE/LDPE blend loaded with 5–8 wt% TiO₂ masterbatch; total thickness for silage clamp covers is 0.10–0.25 mm, while 0.20–0.50 mm sheet is converted into greenhouse blackout and ground-cover applications. UV stabilization uses 0.30–0.60 wt% high-molecular-weight HALS masterbatch in the outer layers because sheet exposed to more than 800 h of QUV-A under ISO 4892-3 should retain at least 50% of original elongation. Mechanical acceptance data are generated under ISO 527-3 for tensile properties and ISO 6383-2 for tear resistance; silage oxygen barrier claims are qualified by ASTM D3985 at 23°C and 0% RH, though published data for this specific Marlex® 7104/black-white structure is limited and must be confirmed by a film permeability trial. Extrusion uses a flat-die line with die width up to 6.0 m and melt temperature 210°C–235°C; the first chill roll is held at 60°C–75°C to prevent the black layer from differential shrinkage that induces curl greater than 5 mm/m. Products include silage clamp covers, bunker silo sheets, white-on-black mulch, fumigation barrier, and greenhouse light-deprivation covers.
Marlex® 7104 is used at 100 phr with 10–30 wt% clean internal edge-trim regrind in industrial dunnage sheet from 1.5 mm to 4.0 mm. Where electrostatic discharge is controlled, antistatic masterbatch is metered at 1.0–3.0 wt% to bring surface resistivity into 10^9–10^11 Ω/sq under ASTM D257; the antistat package should be pre-dispersed in an LLDPE carrier with melt index within 0.20 g/10 min of the base resin to prevent localized resistivity streaks at the die lip. Flat-die extrusion runs at 210°C–235°C, and the vertical three-roll stack is held at 65°C–80°C; roll-stack alignment wedge pressure varied more than 0.05 mm across the web produces sheet bow above 5 mm per linear meter after slitting. Downstream conversion on shuttle or rotary thermoformers requires sheet surface temperature of 120°C–135°C, plug assist speed below 250 mm/s, and mold temperature of 20°C–40°C; cycle times for 2.0 mm dunnage trays are typically 8–20 s. Terminal products include returnable dunnage trays, layer pads for automotive stamping, divider sheets for glass container handling, pallet top frames, and protective interleaving. The material is not food-contact compliant when reprocessed scrap exceeds 15 wt% unless the converter re-validates under FDA 21 CFR 177.1520(c).
Secondary containment liner extrusion uses Marlex® 7104 as a 100 phr base with 2.0–3.0 wt% carbon black masterbatch and 0.20–0.40 wt% antioxidant/acid neutralizer masterbatch; post-consumer regrind is excluded from the formula because contaminant carryover changes chemical resistance stability and weld fusion. The sheet is produced at 1.0–3.0 mm through a flat die with melt temperature 215°C–235°C and textured chill rolls at 65°C–85°C to create a rough surface for concrete adhesion or anchor profile. Chemical resistance screening follows ASTM D543 immersion practice; tensile yield retention after 30 days in representative acid, alkali, and hydrocarbon media is specified by the end user, and published data for Marlex® 7104 under all immersion environments is limited, so a plant-specific coupon program is required before final liner release. Installation geometry references EPA 40 CFR 264.193 where chemical storage bunds must contain 10% of total tank volume or 100% of the largest tank, whichever is greater. Field seaming uses hot wedge welding at 250°C–300°C; weld strength is checked by ASTM D6392 peel and shear, while vacuum box continuity is performed under ASTM D5820 for installations requiring leak testing. Terminal products include concrete bund liners for chemical storage, secondary containment sump liners, reactor containment area membranes, and acid/alkali tank linings. The product envelope excludes service with concentrated oxidizing acids above 40°C unless an oxidation-resistant protective cap layer is coextruded.
Competitive Chevron Phillips Marlex® 7104 LLDPE Sheet Extrusion prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chevron Phillips Marlex® 7104 LLDPE Sheet Extrusion is an ethylene/α-olefin linear low-density polyethylene supplied for flat-die sheet extrusion and subsequent plug-assist or drape thermoforming. The product is characterized by a nominal density of 0.918 g/cm³ under ASTM D1505 and a melt index of 1.0 g/10 min under ASTM D1238 at 190 °C/2.16 kg. These two measurements define the practical processing window and the mechanical response of the formed article. The 1.0 g/10 min melt index places the resin in a low-flow class compared with LLDPE cast-film grades of 2.0 g/10 min to 4.0 g/10 min; the lower melt flow raises melt strength and web stability during vertical draw and radiant-oven sag cycles. The 0.918 g/cm³ density limits crystallinity to a level that retains flexibility and dart impact at the expense of modulus when compared with HDPE sheet grades having densities above 0.940 g/cm³.
Density is controlled by comonomer incorporation. At 0.918 g/cm³, the crystalline mass fraction is lower than HDPE sheet resins and higher than ultralow-density ethylene copolymers. This crystallinity level directly affects flexural modulus, which is measured under ASTM D790 as 0.30 GPa, and limits continuous load-bearing use. The short-chain branch distribution also influences environmental stress crack resistance. In sheet applications exposed to detergents, wetting agents, or lipid-based materials, LLDPE grades with higher α-olefin content commonly outperform LDPE and HDPE in slow-crack-growth tests under ASTM D1693, but the converter must validate the specific forming history because residual stress from roll-stack cooling can reduce field performance irrespective of resin-level ESCR.
| Property | Test method | Typical value |
|---|---|---|
| Density | ASTM D1505 | 0.918 g/cm³ |
| Melt index | ASTM D1238, 190 °C/2.16 kg | 1.0 g/10 min |
| Tensile yield strength | ASTM D638, 50 mm/min | 10.3 MPa |
| Elongation at break | ASTM D638, 50 mm/min | >800% |
| Flexural modulus, 1% secant | ASTM D790 | 0.30 GPa |
| Vicat softening temperature | ASTM D1525, 1 kg | 92 °C |
These values are nominal supplier data derived from compression-molded plaques or specified test specimens and should not be interpreted as lot-release limits. Acceptance testing must use lot-specific certificates of analysis. The polymer’s linear backbone has a smaller degree of long-chain branching than autoclave or tubular LDPE. As a result, die swell is lower, shear thinning is less pronounced, and melt pressure response is steeper with increasing screw speed. These differences require processor control of die-lip temperature and screw-torque limits rather than reliance on historical LDPE settings.
The resin’s 1.0 g/10 min melt index sets a practical die-lip melt-temperature band of 204 °C to 232 °C. Below 204 °C, elevated melt viscosity raises screw torque, increases residence time in the compression zone, and raises the probability of sharkskin surface defects on polished roll surfaces; above 232 °C, oxidative chain scission becomes measurable during extended hold times, producing gel particles that appear as optical defects in finished sheet. Barrel temperature profiles should progress from 160 °C in the feed throat to 204 °C at the metering section, with adapter and die-body zones maintained at 204 °C to 221 °C. These set points are not universal; they must be adjusted to screw diameter, L/D ratio, shotresidence time, and available die-pressure capacity.
Extruder hardware capable of processing the grade includes single-screw machines with L/D ratios of 24:1 to 33:1, barrier screws, and compression ratios between 2.8:1 and 3.5:1. LLDPE melts are less shear-thinning than branched LDPE, so screw-speed increases generate a steeper rise in melt pressure and motor load. Operators should record melt-pressure behavior at the die inlet and use melt-temperature probes rather than relying on barrel temperature set points alone. Filtration before the die is required to capture gel aggregates and foreign particles. A breaker-plate pack of 60/80/100-mesh screens is commonly used; a sustained pressure-drop increase of more than 0.7 MPa from a clean-pack baseline indicates screen blinding and requires replacement to avoid gauge variation.
On sheet lines equipped with gravimetric feeders and direct thickness scanning, the polymer’s lower shear sensitivity compared with LDPE means that die-lip adjustments are less effective in correcting cross-web thickness. Melt-temperature uniformity and die-bolt profiling control gauge. Pre-drying is not normally required for polyethylene, but pellets stored in unheated silos at relative humidity above 60% or transferred through cold-to-heated environments can condense surface moisture. Surface moisture is removed with a hopper dryer operating at 60 °C to 80 °C for 2 h; without drying, the sheet may exhibit pinholes, splay, or irregular gloss when water vaporizes at the die lip.
Roll-stack temperature control is a further boundary condition. Three-roll polishing stacks with chrome-plated rolls typically operate at 60 °C to 90 °C. Roll temperatures below 60 °C can produce chill marks and low-gloss regions, while temperatures above 90 °C can cause the sheet to stick to the roll surface. Air knife or vacuum contact assists transfer from the die lip onto the roll stack and reduces air entrapment. Sheet thickness tolerance on automatic gauge-control lines can be maintained at ±5%, while manual lines commonly exhibit ±10% cross-web variation when die-bolt adjustment is not active.
Direct substitution into an LDPE sheet line is not a drop-in change. Because Marlex® 7104 has a linear backbone and a narrower molecular weight distribution than free-radical LDPE, it develops higher shear viscosity at comparable melt index. On the same die and barrel settings, head pressure may increase, and the extruder drive amperage may reach its limit before target output is achieved. A die-temperature increase of 5 °C to 10 °C is often required to match backpressure when changing from a branched LDPE of 0.922 g/cm³ and 1.0 g/10 min. The lower die swell of the LLDPE also requires a die gap set closer to final sheet gauge than would be used for LDPE.
In exchange, the LLDPE yields measurably higher dart impact and tear propagation resistance at equivalent sheet thickness. Per ASTM D1709 falling-dart tests on 0.5 mm sheet, the resin performs within the expected range for LLDPE but published data for this specific configuration is limited; the supplier’s technical bulletin should be consulted for exact impact values. The higher extensional viscosity reduces web sag during radiant-oven heating, permitting a wider processing window for deep-draw thermoforming than low-MI LDPE or high-MI LLDPE film grades. Compared with high-MI LLDPE grades of 2.0 g/10 min to 4.0 g/10 min, Marlex® 7104 is less suitable for thin cast film below 50 µm, where high-shear flow through a narrow die gap is limiting, but it is more suitable for sheet from 0.25 mm to 6.0 mm, where melt strength maintains gauge consistency.
In plug-assisted thermoforming of 1.0 mm to 3.0 mm sheet, infrared heating is typically set to bring the sheet surface to 130 °C to 150 °C. Below 125 °C, radial thinning at the plug contact region increases; above 155 °C, localized sag and surface oxidation can cause defects. Mold temperatures between 20 °C and 60 °C provide sufficient cooling for amorphous polyethylene sheet, with cycle time controlled by contact pressure and part thickness. Wall-thickness distribution in a 2:1 draw ratio part typically declines to 40% to 50% of the starting sheet thickness at the bottom corner; the narrow molecular weight distribution of LLDPE maintains more uniform thickness than LDPE at equivalent draw ratios in published processing studies, but exact distribution depends on plug geometry, speed, and sheet temperature uniformity.
The Vicat softening temperature of 92 °C under ASTM D1525 provides an upper bound for short-term contact with heated surfaces. Continuous-use temperature is lower because modulus decays as the polymer approaches its crystalline melting range. A practical continuous-use limit for unstabilized LLDPE sheet is approximately 60 °C; exact values depend on sheet thickness, cooling rate, and annealing history. Extruded sheet cooled on a three-roll stack retains residual orientation and cold-crystallizes unevenly. Longitudinal shrinkage can reach 1% to 2% when sheet is post-heated to 80 °C for 30 min, unless the roll-stack speed is adjusted to reduce draw or an annealing zone is used. Cut parts for thermoforming should be conditioned at the forming temperature to relax orientation before final trimming.
For food-contact sheet, the resin falls under 21 CFR 177.1520 for olefin polymers when the finished sheet meets extractives limitations; the supplier can provide a food-contact statement. In the European Union, the grade is subject to registration under REACH (EC) No 1907/2006, and typical LLDPE formulations do not exceed 2011/65/EU heavy-metal thresholds, but the final compound must be validated by the converter.
| Requirement | Reference | Condition |
|---|---|---|
| U.S. food-contact olefin polymer | 21 CFR 177.1520 | Compliance based on end-use migration testing |
| EU chemical registration | REACH (EC) No 1907/2006 | Monomer and additive registration via supplier |
| Restriction of hazardous substances | 2011/65/EU | No intentional heavy-metal additive |
| Resin identification code | ISO 11469 | PE-LLD |
Post-industrial LLDPE sheet scrap is re-introduced into virgin material at up to 20% by weight in standard single-screw lines without loss of tensile yield under ASTM D638, provided the regrind is free of paper, adhesive, and incompatible polymers. Higher regrind content shifts the melt-index distribution and can move the die-pressure baseline. The grade is not intended for outdoor UV exposure without an additive package; unstabilized sheet exhibits chalking and loss of elongation under ASTM D638 after outdoor weathering, so converters must specify a UV-stabilized formulation if the finished part is exposed to sunlight.