| HS Code | 315943 |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene-1 |
| Density | 0.918 g/cm³ |
| Melt Index 190 C 2 16 Kg | 0.9 g/10 min |
| Melting Point | 118 °C |
| Vicat Softening Point | 95 °C |
| Tensile Strength At Yield Md | 1500 psi |
| Tensile Strength At Yield Td | 1400 psi |
| Tensile Strength At Break Md | 4500 psi |
| Tensile Strength At Break Td | 4000 psi |
| Elongation At Break Md | 600% |
| Elongation At Break Td | 700% |
| Elmendorf Tear Strength Md | 250 g |
| Elmendorf Tear Strength Td | 400 g |
| Dart Drop Impact | 200 g |
| Haze | 10% |
| Gloss 45 | 60% |
| Secant Modulus 1 | 30000 psi |
| Puncture Resistance | 50 J/cm |
| Heat Seal Initiation Temperature | 105 °C |
| Water Vapor Transmission Rate | 0.5 g/100 in²/24h |
| Oxygen Transmission Rate | 100 cc/100 in²/24h |
| Escr | >1000 h |
| Molecular Weight Distribution | Narrow |
As an accredited Chevron Phillips MarFlex® 7109CL LLDPE Blown Film Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Chevron Phillips MarFlex® 7109CL LLDPE Blown Film Resin is packaged in 25 kg bags, available on pallets or in bulk. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with palletized 25 kg bags of Chevron Phillips MarFlex® 7109CL LLDPE Blown Film Resin, securely stretch-wrapped. |
| Shipping | Chevron Phillips MarFlex® 7109CL LLDPE Blown Film Resin is not regulated for transport under DOT, IATA, IMDG, or ADR. It is shipped as solid pellets in 25-kg bags, 1,000-kg bulk bags, or bulk trucks/railcars. Keep containers closed and protect from moisture, heat, and prolonged sunlight. |
| Storage | Store Chevron Phillips MarFlex® 7109CL LLDPE Blown Film Resin in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, ignition sources, moisture, and contaminants. Keep original packaging closed and palletized; avoid excessive stacking or damaging bags. Protect from UV exposure and extreme temperatures. Follow the manufacturer’s SDS and local regulations for safe handling, inventory rotation, and spill cleanup. |
| Shelf Life | Recommended shelf life is 12 months from manufacture when stored in original unopened packaging at ambient temperatures below 50°C (122°F). |
Monofilm lines running MarFlex 7109CL at film thicknesses of 150–200 µm typically use a weight-fraction formulation of 65–70 wt% MarFlex 7109CL, 20–25 wt% LDPE with melt index 0.25 g/10 min (ISO 1133-1:2022), 5–10 wt% HDPE with density 0.956 g/cm³, and 2–3 wt% carbon black masterbatch containing 40% carbon black dispersed in an LLDPE carrier. The LDPE addition raises melt strength and stabilizes the bubble, while HDPE improves stiffness and tear propagation resistance. Compliance for bags used in transport of dangerous goods is defined by UN Model Regulations Chapter 6.5 for FIBCs and Chapter 6.1 for sacks; the film must pass drop, stacking, and tear tests specified in the relevant packing instruction. Mechanical property claims are anchored to ASTM D1709 dart impact, ASTM D1922 Elmendorf tear, and ASTM D882 tensile. On a production line retrofitted with a 75 mm grooved-feed extruder, L/D 30:1 barrier screw, and a 450 mm spiral mandrel die with die gap set to 2.0 mm, bubble instability is observed as frost line oscillation when the blow-up ratio exceeds 3.0:1 at melt temperatures above 220°C. Internal bubble cooling and a high-stalk bubble geometry with a frost line height of 8–10 die diameters reduce this instability. Processing above 240°C creates localized oxidative degradation and gel formation that subsequently reduces dart impact strength and increases draw resonance risk at the oscillating haul-off. Terminal products include FIBC inner liners, valve sacks for polyolefin pellets, and chemical powder sacks for cementitious materials.
In three-layer coextruded structures for frozen vegetables, the sealant layer contains 85 wt% MarFlex 7109CL, 10 wt% LDPE, 3 wt% antiblock masterbatch (diatomaceous earth, 20% active in LDPE carrier), and 2 wt% slip masterbatch (erucamide, 5% active in LLDPE carrier). Food-contact compliance is established under FDA 21 CFR 177.1520(c)3.2a for olefin polymers and EU Regulation 10/2011 with overall migration limit 10 mg/dm² per EN 1186 test methods. The production process uses a three-layer blown film line with two 55 mm extruders for skin layers and one 65 mm extruder for the core, feeding a 300 mm spiral mandrel die with 1.8 mm die gap. The bubble is maintained at a blow-up ratio of 2.2:1 and a melt temperature of 210°C; frost line height is kept at 6 die diameters to minimize migration of erucamide to the outer film surface before winding. Failure modes in production include blocking on the collapsing frame when slip additive concentration exceeds 1,200 ppm active erucamide, and low hot-tack strength per ASTM F1921 when the skin layer contains more than 5 wt% antiblock masterbatch that disrupts seal continuity. Corona treatment is applied to the outer layer at 38–42 mN/m surface energy, but the sealant side is left untreated because treatment generates surface carboxyl groups that reduce heat-seal strength. Terminal products include frozen vegetable bags, ice cream pillow pouches, and seafood vacuum skin packaging films, all typically in the 40–60 µm thickness range.
Agricultural silage bale wrap produced at 25 µm thickness requires a formulation of 88 wt% MarFlex 7109CL, 8 wt% low-molecular-weight tackifier masterbatch (polyisobutylene, 50% active in LLDPE carrier), and 4 wt% UV/HALS masterbatch containing hindered amine light stabilizers at 10% active concentration. Compliance is referenced to EN 13207:2018 for thermoplastic silage films and to EN ISO 527-3 for film tensile properties. The blown film process uses a 65 mm extruder with L/D 28:1 and a 400 mm die with 1.5 mm die gap; the blow-up ratio is 3.0:1 and melt temperature is 200°C. The polyisobutylene migrates to the surface during winding; published data for this specific tackifier-load configuration is limited, but typical production targets fall within a peel cling range of 2.5–3.5 N per ASTM D5458 after 24 h aging. Excessive tackifier loads above 10 wt% masterbatch cause reel blocking and slitting buildup on the NIP rollers. A process conflict arises from the requirement of high tear propagation resistance in the machine direction: the film is oriented by a pre-stretch unit at 60–70% elongation during wrapping, and orientation-induced crystallinity increases stiffness, which is measured as secant modulus per ISO 527-3. Terminal products include round bale silage wrap, oxygen-barrier silage sheets in 150 µm thickness, and green cover films for chopped maize storage; all require UV stability of at least 12 months outdoor exposure per EN 13207 accelerated weathering methods.
In construction-grade sheeting applications, the blend is 97 wt% MarFlex 7109CL and 3 wt% carbon black masterbatch (38% active carbon black) extruded to a nominal thickness of 150 µm (6 mil). Compliance is anchored to ASTM E1745 for plastic water vapor retarders used in contact with soil or granular fill under concrete slabs, which requires Class A vapor retarder permeance not exceeding 0.1 perm under ASTM E96 Method B, and to ASTM D4397 for polyethylene sheeting intended for construction, industrial, and agricultural applications, requiring minimum tensile strength of 8.3 MPa and elongation at break of 300% per ASTM D882. Production uses a 90 mm grooved-feed extruder with a 700 mm die and 2.4 mm die gap; the blow-up ratio is 3.2:1 and the bubble is collapsed through a tri-fold winding system that produces slit widths of 3–6 m. Gauge variation across the web is controlled by oscillating haul-off with a ±5% thickness tolerance; deviation beyond 5% creates thin spots that fail puncture resistance under ASTM D1709 and reduces vapor barrier integrity under ASTM E96. Operational boundaries include avoiding installation in direct sunlight beyond 90 days because the carbon black masterbatch provides only 6–12 months UV weathering resistance, which is insufficient for permanent exposure; additionally, the sheet must not be used with solvent-based adhesives or in contact with aromatic hydrocarbons that swell polyethylene and increase permeance. Terminal products include under-slab vapor retarders, crawl space encapsulation liners, and temporary concrete curing covers.
High-speed stretch hood pallet stabilization lines running 70–100 cycles per hour convert a monolayer blown film formulation of 75 wt% MarFlex 7109CL, 15 wt% LDPE with melt index 0.30 g/10 min, and 10 wt% polyisobutylene tackifier masterbatch (25% active in LLDPE carrier). The compliance standard for cling performance is ASTM D5458 peel cling, and tensile properties are measured by ISO 527-3; the resin must be registered under REACH Regulation (EC) No 1907/2006 for industrial use. Production equipment includes a 120 mm extruder with L/D 32:1 and a 650 mm oscillating die with 2.2 mm die gap; the bubble is run at a blow-up ratio of 4.0:1 to achieve balanced MD/TD tear properties. The film is stretched in the hooder unit at 60–80% elongation during application, and failure modes on the line include film puncture at the pallet corners when the film thickness is below 80 µm, and elastic recovery loss when the LLDPE content exceeds 80 wt% because excessive linear crystallinity reduces the stretch holding force. Published data for this specific LLDPE/PIB blend is limited; a die gap must not be reduced below 1.8 mm or the shear rate at 120 s⁻¹ causes melt fracture on the outer surface, while too wide a gap reduces directional orientation and lowers yield strength. Terminal products include stretch hood films in thicknesses of 80–150 µm, pallet stabilizers for appliance distribution, and anti-collapse films for beverage tray stacking.
Although can liner film is a low-differentiation application, the blend of 70 wt% MarFlex 7109CL, 25 wt% post-industrial LLDPE reclaim, and 5 wt% calcium carbonate masterbatch (60% active in LDPE carrier) is extruded at 30 µm thickness on a high-output monofilm line equipped with a 100 mm extruder and twin-station surface winder. Compliance is limited to physical property specifications: ASTM D1709 dart impact, ASTM D1922 Elmendorf tear, and ASTM D882 tensile. The melt temperature is maintained at 210°C, the die gap at 2.0 mm, and the blow-up ratio at 3.0:1. Terminal products include kitchen trash bags, office can liners, and janitorial cart liners. Published data for this specific reclaim-containing configuration is limited; substitution of reclaim above 25 wt% increases gel particle formation and reduces dart impact consistency across production shifts.
Competitive Chevron Phillips MarFlex® 7109CL LLDPE Blown Film Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chevron Phillips MarFlex® 7109CL is a linear low-density polyethylene blown film resin supplied in pellet form for monolayer and coextruded film structures. The nominal resin density is 0.918 g/cm³ when tested in accordance with ASTM D1505, and the nominal melt index is 1.0 g/10 min as measured at 190 °C under a 2.16 kg load per ASTM D1238 or ISO 1133-1:2022. The product is specified for high-clarity blown film applications in which optical uniformity, seal integrity, and tear resistance are processed simultaneously on bag-making equipment. Typical end uses include fresh produce packaging, bakery overwrap, garment bags, and thin-gauge food-contact films. Processing commonly occurs at a blow-up ratio of 2.0:1 to 3.0:1 and a melt temperature between 190 °C and 230 °C.
Film performance is line-dependent and is evaluated on blown film samples of controlled gauge, usually 25 µm, after fixing blow-up ratio, die gap, and frost line height. Direct comparison with other resins therefore requires matched fabrication conditions rather than reliance on isolated resin properties.
Compared with general-purpose butene-copolymer LLDPE film resins of equivalent density and melt index, 7109CL is modified to reduce wide-angle scattering and improve surface gloss while retaining the extrusion processability of a conventional linear resin. Published comparative data indicate that conventional butene LLDPE grades frequently exhibit haze values of 12% to 18% at 25 µm under ASTM D1003, whereas 7109CL is supplied against a typical haze target below 10% on the same gauge. The improvement is achieved without the higher melt pressure and die-lip deposit formation commonly associated with metallocene-catalyzed LLDPE grades, but the trade-off is a lower dart impact value than many mLLDPE film resins. On continuous blown film lines, that trade-off is measured through dart drop under ASTM D1709A and Elmendorf tear under ASTM D1922, rather than through single-point clarity readings alone.
The resin is frequently selected when film converters require an optical surface closer to LDPE but want to avoid the higher crystallinity-driven stiffness and lower tensile strength of an LDPE-rich blend. In comparison with LDPE, 7109CL has a more linear backbone and lower melt tension, which requires different bubble geometry control. LDPE is sometimes added at 10 wt% to 20 wt% to increase bubble stability on narrow-die lines; however, haze increases as the LDPE fraction exceeds 15 wt% because of density and crystallinity differences. Published data for this specific blend configuration is limited, so production trials should verify the optical target with a fixed 2.5:1 blow-up ratio.
Property values in the following table are compiled from typical grade data and are not specification limits. They are generated on 25 µm monolayer blown film with a 2.5:1 blow-up ratio, 2.0 mm die gap, and 205 °C melt temperature. The certificate of analysis is the governing document for lot-specific results.
| Property | Test method | Nominal value | Unit |
|---|---|---|---|
| Resin density | ASTM D1505 | 0.918 | g/cm³ |
| Melt index at 190 °C, 2.16 kg | ASTM D1238 | 1.0 | g/10 min |
| Tensile strength at break, MD | ASTM D882 | 48 | MPa |
| Tensile strength at break, TD | ASTM D882 | 40 | MPa |
| Elongation at break, MD | ASTM D882 | 650 | % |
| Elongation at break, TD | ASTM D882 | 750 | % |
| Secant modulus at 1%, MD | ASTM D882 | 190 | MPa |
| Secant modulus at 1%, TD | ASTM D882 | 210 | MPa |
| Dart drop impact, Method A | ASTM D1709A | 120 | g |
| Elmendorf tear, MD | ASTM D1922 | 360 | g |
| Elmendorf tear, TD | ASTM D1922 | 480 | g |
| Haze | ASTM D1003 | 8 | % |
| Gloss at 60° | ASTM D2457 | 65 | — |
Processing of 7109CL on monolayer blown film lines is typically performed with single-screw extruders having a 24:1 to 30:1 L/D ratio, barrier-flight screws, and grooved feed sections to suppress screw slip at high backpressure. Die gap is set between 1.5 mm and 2.5 mm; die gaps below 1.2 mm may raise melt pressure and produce surface melt fracture on 100 mm dies, while die gaps above 2.5 mm dilute transverse orientation. Melt temperature measured at the adapter is usually maintained between 190 °C and 230 °C. At temperatures above 250 °C, oxidative chain scission and gel formation can occur, producing optical defects and screen-pack plugging. A production-scale symptom of insufficient bubble cooling is a frost line height below 5 die diameters, which has been associated with gauge bands and lower transverse Elmendorf tear. Raising the frost line to 5 to 7 die diameters and balancing the dual-lip air ring improve gauge uniformity at 2.5:1 blow-up ratio.
The resin’s comparatively low melt tension relative to LDPE requires controlled air-ring flow. Excessive internal bubble cooling can collapse the bubble if the frost line is positioned too high. On a 65 mm grooved-feed extruder, output typically falls within 1.2 kg/h to 1.6 kg/h per centimetre of die circumference, but this range depends on screw design, die gap, and melt temperature. Melt pressure at the screen changer is generally maintained below 350 bar to avoid excessive shear heating; continuous pressure above 400 bar may signal screen blockage or an undersized die gap. Lot-to-lot control is centred on melt index and resin density because these parameters drive film gauge and optical uniformity. A shift of 0.1 g/10 min in melt index can alter extruder melt pressure by an estimated 5% to 10% on a fixed die gap, so processors commonly set incoming material acceptance windows for both density and melt index.
Heat-seal behaviour is evaluated with flat-bar or rotary sealing equipment according to ASTM F88 or ASTM F2029. For thin LLDPE food-packaging films, seal initiation is commonly determined on the finished film rather than on the resin alone because seal-bar pressure, dwell time, and film gauge shift the initiation temperature. Converters running vertical form-fill-seal lines often require hot-tack strength sufficient to hold product weight during the sealing cycle; this is assessed with ASTM F1921. The resin’s seal curve is typical for a butene-copolymer LLDPE, with stable seals in the range of 100 °C to 140 °C. Published data for this specific configuration is limited, so line-specific seal curves must be generated for each packaging structure.
Corona treatment of the film surface to 38 dyn/cm to 42 dyn/cm, measured by ASTM D2578, is standard for flexographic or rotogravure print adhesion. Because polyethylene is nonpolar, ink anchorage depends on surface oxidation. Values below 36 dyn/cm often produce poor wet-out and variable print quality on high-speed presses. This is not a resin-specific limitation, but it must be controlled when 7109CL is used in printed produce bags or laminated structures.
In coextrusion, 7109CL is frequently placed in the skin layer where its optical contribution is greatest. A skin-layer thickness of 10 µm to 15 µm on a 50 µm total structure is generally sufficient to reduce haze, while the core layer retains a lower-cost fractional-melt LLDPE or recycled material. Layer ratio control is critical because a skin layer below 10% of total thickness may produce non-uniform surface coverage and optical striping. The resin can also be blended with mLLDPE at low levels to raise dart impact, but the blend may increase extrusion pressure and die-lip deposit formation. Published data for specific mLLDPE/7109CL blend ratios is limited; line trials are required to establish an acceptable balance between optics, bubble stability, and extruder amperage.
Food-contact use of 7109CL is governed by the base olefin polymer status under FDA 21 CFR 177.1520(c), with end-use extraction testing on the finished article. Under EU Regulation (EC) No 10/2011, overall migration and specific migration limits must be verified on the final film after corona treatment, printing, and lamination; resin compliance alone does not cover these post-processing steps. For REACH registration and RoHS heavy-metal restrictions, the supplier’s regulatory datasheet should be retained as part of incoming inspection records.
Moisture absorption in LLDPE is low; pre-drying is generally not required unless the pellets have been exposed to direct condensation or outdoor storage at relative humidity above 60%. In such cases, a desiccant hopper dryer at 60 °C to 70 °C for 2 h to 4 h is applied. Reclaimed scrap should be kept free of polypropylene, EVOH, or paper fibre contamination because melt-phase incompatibility creates gel-like specks that degrade haze and dart impact. Inventory rotation under first-in-first-out discipline limits oxidative yellowing during extended warehousing.