| HS Code | 174377 |
| Productname | Chevron Phillips Dynex™ D508A Enhanced LLDPE Blown Film Resin |
| Polymertype | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Hexene-1 |
| Meltindex 190c 2 16kg | 0.8 g/10 min |
| Density | 0.919 g/cm³ |
| Meltingpoint | 122 °C |
| Vicatsofteningpoint | 100 °C |
| Tensilestrengthatbreak Md | 5,400 psi |
| Tensilestrengthatbreak Td | 5,000 psi |
| Elongationatbreak Md | 600% |
| Elongationatbreak Td | 700% |
| Elmendorftearstrength Md | 300 g |
| Elmendorftearstrength Td | 500 g |
| Dartdropimpact F50 | 200 g |
| Haze | 12% |
| Gloss 45degree | 55 |
| Coefficientoffriction | 0.2 |
As an accredited Chevron Phillips Dynex™ D508A Enhanced LLDPE Blown Film Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Chevron Phillips Dynex™ D508A is packaged in 25 kg (55 lb) polyethylene bags, palletized, and available in bulk trucks or railcars. |
| Container Loading (20′ FCL) | 20′ FCL container loading: Chevron Phillips Dynex™ D508A Enhanced LLDPE Blown Film Resin, securely packed and stowed for ocean transport. |
| Shipping | Chevron Phillips Dynex™ D508A Enhanced LLDPE Blown Film Resin is typically shipped in 25 kg polyethylene bags, palletized and stretch-wrapped, or in bulk trucks/railcars. It is a non-hazardous polymer; store dry, covered, away from heat, moisture, and direct sunlight. Follow carrier and local regulations. |
| Storage | Store Dynex™ D508A in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, flames, and strong oxidizers. Keep material in original, sealed, labeled containers or bags, palletized and off the floor. Prevent moisture, dust, and contamination. Use first-in, first-out stock rotation. Avoid excessive stacking and prolonged high temperatures. Follow local regulations and SDS recommendations. |
| Shelf Life | Two years from date of manufacture when stored unopened in original packaging under cool, dry, well-ventilated conditions away from direct sunlight. |
D508A is charged to three-layer blown film lines at a nominal density of 0.920 g/cm³ and melt index of 0.85 dg/min as determined under ASTM D1238 at 190°C/2.16 kg. The grade is specified against ASTM D4976-21 for polyethylene film and molding resins, and food-contact construction is documented under 21 CFR 177.1520(c) when the finished sack is used for indirect food contact. In heavy-duty chemical sack formulations, D508A is loaded at 70–85 wt% in the core and intermediate layers, while LDPE homopolymer with melt index 0.3–1.0 dg/min and density 0.920–0.922 g/cm³ is used at 10–20 wt% in outer layers to widen heat-seal latitude. UV-stabilized export grades add a HALS/UV masterbatch at 3–5 wt%, and slip/antiblock concentrates are used at 1–2 wt% only where sack surface separation is required. Pellets are not hygroscopic, but pre-drying at 70–80°C for 2–3 h is required when hopper condensation occurs at ambient RH above 60%; failure to dry surface condensation produces pinhole-generating steam volatilization at the die. Conversion on 350–500 mm spiral mandrel dies uses die gaps of 2.0–2.4 mm, blow-up ratios of 2.5:1–3.0:1, and melt discharge temperatures of 204–218°C; frost line is held at 600–800 mm above the die face to balance bubble stability and orientation. Die shear rates commonly fall in the 100–500 s-1 range under these conditions. On production-scale lines, raising blow-up ratio above 3.5:1 produces gauge variation in the ±8% range and a measurable loss of machine-direction Elmendorf tear as tested by ASTM D1922, while cooling too rapidly lowers dart impact under ASTM D1709-16a Method A. Regrind from trimmed edges is reprocessed at 10–15 wt% without yield loss but may increase gel-related surface defects when die gaps fall below 2.0 mm. Contamination by polypropylene regrind above 2 wt% is avoided because it reduces low-temperature dart impact through phase incompatibility. Terminal products include gusseted chemical sacks from 125–200 µm, liners for corrugated bulk boxes, and valve sacks for resin and mineral powder filling.
Agricultural silage clamp covers and bale wraps are produced from D508A in monolayer or three-layer constructions with a finished thickness of 150–250 µm. Compliance for such films is anchored to EN 13207:2018, which specifies tensile and tear requirements for silage films before and after exposure. Formulation loadings in three-layer covers place D508A at 90–98 wt% in the core, with a UV-stabilizer masterbatch at 2–5 wt%; black covers intended to suppress light transmission and surface growth incorporate carbon black concentrate at 4–6 wt%, yielding 2.0–2.5 wt% carbon black in the final film. Where punctures from corn stubble or forage stems are a chronic field failure, converters blend 5–10 wt% of an EVA with vinyl acetate content of 8–12% into the skin layers to increase low-elongation puncture resistance. Processing is run on dies of 600–1000 mm with die gaps of 2.2–2.6 mm, blow-up ratios of 3.0:1–3.5:1, and melt temperatures of 190–210°C. High-stalk bubble cooling lengthens the quench zone to 500–700 mm above the die and increases transverse orientation, which raises tear propagation resistance as determined by ISO 6383-2. Low blow-up ratio below 2.5:1 drops transverse tear significantly, while exceeding 3.5:1 destabilizes the bubble when ambient air temperature fluctuates more than 10°C during a shift. Batch-to-batch dart impact variation in silage film production is commonly held within ±8% when silo reclaim and edge trim feed streams are held below 15 wt%. Terminal products are clamp silage covers, round and square bale wrap, and bunker silo top sheets.
Substitution of conventional butene-LLDPE with D508A in frozen-food blown film shifts the low-temperature dart-impact response and permits downgauging without losing drop resistance. The food-contact compliance file includes 21 CFR 177.1520(c) with Conditions of Use E through G for refrigerated and frozen food, and European construction is assessed under Regulation (EU) No 10/2011, Annex I and II, with an overall migration limit of 10 mg/dm² into food simulants. Frozen vegetable bag formulations load D508A at 90–100 wt%, with 0–8 wt% mLLDPE of density 0.912–0.918 g/cm³ and melt index 1.0–2.0 dg/min added only when lower seal initiation is required. Slip masterbatch based on erucamide is added at 1–3 wt%, and synthetic silica antiblock concentrate is added at 0.5–1.5 wt% to prevent blocking at storage temperatures near -20°C. The blown film equipment typically uses 45–65 mm extruders with L/D ratios of 24:1–30:1, die gaps of 1.5–2.0 mm, blow-up ratios of 2.0:1–2.5:1, and melt temperatures of 193–204°C; lower melt temperature reduces oxidative gel formation and preserves organoleptic neutrality. Line operators monitor die lip edge buildup because an 0.85 dg/min melt index resin at low temperatures can exhibit high melt viscosity and increased backpressure on shallow-channel screws. Finished film is corona-treated to 38–42 mN/m for ink adhesion, and tensile properties are verified by ASTM D882-18 before slitting. Published data for low-temperature dart impact of D508A at -20°C in this specific film structure are limited, so converter-run abuse tests using ASTM D1709-16a Method A are performed before customer qualification. Terminal products include ice bags, frozen vegetable pouches, frozen meat overwrap, and bag-in-box liners.
| Scenario | Compliance or Test Standard | Designation / Clause | Controlled property |
|---|---|---|---|
| Heavy-duty chemical sacks | ASTM D1709-16a Method A; ASTM D1922; ASTM D882-18 | Dart impact, Elmendorf tear MD/TD, tensile break strain | Gauge-specific drop resistance and tear anisotropy |
| Silage covers | EN 13207:2018; ISO 6383-2 | Silage film type and weathering classification; Elmendorf tear | Retained tensile elongation and tear after exposure |
| Frozen-food film | 21 CFR 177.1520(c); Regulation (EU) No 10/2011 | Annex I; overall migration 10 mg/dm² | Food-contact compliance and organoleptic neutrality |
| Stretch hood | ASTM D5748-19; EUMOS 40509 | Probe puncture; unitized load rigidity | Puncture force and load containment under transport |
In drum-liner conversion, D508A is processed at low blow-up ratios to preserve machine-direction tear and to limit crease splitting during insertion into steel and fibre drums. Chemical compatibility is assessed under 49 CFR 173.24(e) when the liner is used as inner packaging for hazardous materials, and non-hazardous industrial liners are tested for environmental stress-crack resistance by ASTM D1693 Condition C. Clear drum liners are run at 100 wt% D508A; black or antistatic solvent-service liners incorporate 2–4 wt% conductive carbon black or antistatic masterbatch. The film thickness range is 200–400 µm, requiring die gaps of 2.5–3.0 mm and melt temperatures of 204–221°C to prevent melt fracture at high output. Blow-up ratio is held at 1.8:1–2.2:1 to bias orientation toward the machine direction, which raises tear resistance but reduces transverse tensile strain; this trade-off is acceptable because drum liners are inserted vertically and stressed in the machine direction. Filtration screens of 60–80 mesh are placed before the die to reduce pinhole-generating gels, and internal bubble cooling is used above 250 µm gauge to stabilize the thick-walled bubble. Strong oxidizing acids above 90 wt% concentration at temperatures above 40°C can surface-oxidize the liner; published data for D508A in this specific configuration are limited, so compatibility testing with the actual chemical mixture is required. Terminal products include pail liners, drum liners, tote liners, and corrugated box liners.
Pallet hood film formulations based on D508A are developed around the balance between tensile recovery after extension and puncture resistance under ASTM D5748-19. Load containment is specified by EUMOS 40509, and elastic recovery is often measured by a converter method derived from ASTM D5459. Typical stretch hood formulation loads D508A at 70–85 wt%, with 15–30 wt% mLLDPE of density 0.912–0.918 g/cm³ and melt index 1.0–2.0 dg/min incorporated to lower stiffness and improve recovery after 45–60% elongation. Some medium-elasticity hoods use an EVA with 8–12% vinyl acetate at 10–20 wt%, but no cling agent is added because stretch hoods are heatset and must not block after slitting. The process is high-stalk blown film extrusion with a blow-up ratio of 3.0:1–3.5:1, die gap 1.5–2.0 mm, melt temperature 190–205°C, and frost line held at 8–10 die diameters above the die. The high-stalk configuration builds chain orientation in the transverse direction, increasing dart impact and puncture resistance while preserving low elongation set. Exceeding 3.5:1 blow-up ratio produces bubble instability and thickness bands that cause uneven stretching force when the hood is applied; falling below 3.0:1 reduces transverse tensile strength and hood corner puncture performance. Terminal products include stretch hoods for pallets of bagged cement, insulation materials, and beverage containers, along with dust covers for rack storage.
Coextruded lamination webs for flexible packaging place D508A in the core and sometimes in the sealant layer where stiffness and heat-seal strength must survive adhesive lamination to PET, BOPP, or metallized substrates. Compliance is controlled by Regulation (EU) No 10/2011 for the European market and 21 CFR 177.1520(c) for the United States, with the final laminate tested for overall migration below 10 mg/dm² in the intended food simulants. Formulation for the core layer uses 60–80 wt% D508A with 20–40 wt% LDPE or EVA of vinyl acetate content 4–9% to reduce seal initiation temperature to 90–105°C in the sealant layers. The coextruded film is run at die gaps of 1.5–2.0 mm, blow-up ratios of 2.0:1–2.5:1, and melt temperatures of 193–204°C; controlled frost line at 400–500 mm above the die limits haze and maintains consistent coefficient of friction after slitting. Corona treatment is applied at 38–42 mN/m on the lamination side, and lamination is completed on adhesive-coating equipment with a nip temperature of 65–80°C. Published data for seal initiation of D508A in specific three-layer coextrusions are limited; converter trials are required to set exact layer ratios against substrate gauge. Terminal products include lamination films for stand-up pouches, sachets, and frozen food overwrap structures.
Competitive Chevron Phillips Dynex™ D508A Enhanced LLDPE Blown Film Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chevron Phillips Dynex™ D508A Enhanced LLDPE Blown Film Resin is a pelletized alpha-olefin copolymer supplied for monolayer and coextruded blown film structures in which puncture resistance, tear strength, and seal integrity must be maintained at reduced gauge. The model designation D508A identifies the base resin and an additive package; the additive composition is lot-specific and should be confirmed against the certificate of analysis. The primary purchasing specifications are nominal density and melt index. Nominal density is 0.918 g/cm³ when tested in accordance with ASTM D1505, and nominal melt index is 0.5 g/10 min when tested in accordance with ASTM D1238 at 190 °C/2.16 kg. A typical lot-to-lot melt-index tolerance is ±0.05 g/10 min. For international procurement, the corresponding methods are ISO 1183 for density and ISO 1133-1:2022 for melt mass-flow rate. The crystalline melting peak of a LLDPE in this density class is typically 120–124 °C by ASTM D3418. End uses include heavy-duty sacks, industrial liners, and agricultural films at 25–125 µm thickness.
At equal nominal density, D508A differs from a conventional Ziegler-Natta 0.918 g/cm³ butene LLDPE primarily in molecular architecture and melt index rather than in crystallinity. Conventional butene LLDPE has a broader short-chain branching distribution and, in film extrusion, often yields a less balanced machine-direction/transverse-direction tear profile. The enhanced architecture is intended to shift the failure envelope toward higher ASTM D1709 dart impact and higher ASTM D1922 Elmendorf tear at equal gauge; however, published data for this specific configuration is limited. Secant modulus measured by ASTM D882 is governed primarily by density, so the grade is not a direct substitute for a 0.925 g/cm³ medium-density LLDPE if stiffness is the controlling specification. Against LDPE produced in high-pressure tubular or autoclave processes, D508A has minimal long-chain branching. The practical consequence is lower melt strength and a lower maximum stable blow-up ratio: LDPE often runs at 2.5–4.0:1, while D508A is normally run at 2.0–2.8:1. Against 0.945–0.960 g/cm³ HDPE film resins, D508A shows lower yield stress and tensile modulus but higher Elmendorf tear and lower density.
| Resin class | Nominal density | Nominal melt index | Typical processing range | Primary film property difference |
|---|---|---|---|---|
| D508A enhanced LLDPE | 0.918 g/cm³ | 0.5 g/10 min | BUR 2.0–2.8:1; melt 190–220 °C | Higher dart and more balanced tear than butene LLDPE at equal gauge |
| Conventional butene LLDPE | 0.918 g/cm³ | 0.8–1.0 g/10 min | BUR 2.0–3.0:1; melt 185–215 °C | Lower head pressure and lower dart/tear balance |
| LDPE | 0.917–0.922 g/cm³ | 0.25–2.0 g/10 min | BUR 2.5–4.0:1; melt 150–180 °C | High melt strength and high clarity; lower dart and tear |
| HDPE film | 0.945–0.960 g/cm³ | 0.5–1.2 g/10 min | BUR 3.0–6.0:1; melt 190–230 °C | Higher modulus and moisture barrier; lower tear resistance |
The lower melt index of 0.5 g/10 min also differentiates D508A from general-purpose liner resins supplied at 1.0 g/10 min. The higher molecular weight associated with the lower melt index raises head pressure and reduces melt extensibility but improves dart impact and slow-puncture resistance. Film processors may blend 10–30 wt% LDPE into D508A to recover bubble stability and obtain acceptable gauge uniformity. The blend ratio is not fixed; it is optimized against ASTM D1709 dart impact, ASTM D1922 tear, and capacitance gauge thickness maps. Blending above 30 wt% LDPE can dilute the film property advantages and shift the composition toward LDPE-like mechanical response.
On air-cooled blown film lines, barrel zone settings are typically profiled from 160 °C at the feed throat to 180–200 °C in the metering zone, with die temperatures of 190–210 °C. Melt temperature at the die lip should be held within 190–220 °C. Operation below 185 °C increases melt fracture; sustained operation above 220 °C increases oxidative gel formation and can produce bubble holes. The practical melt temperature band is approximately ±5 °C around 200 °C. Die gap is set in the 1.5–2.5 mm range. A 2.0–2.8:1 blow-up ratio is recommended; below 2.0:1, transverse-direction tear declines, while above 2.8:1, bubble respiration and gauge bands increase. Frost-line height is maintained at 1–3 die diameters; raising the frost line above 3 die diameters causes a sharp loss in transverse-direction tear, and lowering it below 1 die diameter increases blocking and machine-direction tear anisotropy.
| Parameter | Target | Measurement method or equipment |
|---|---|---|
| Die gap | 1.5–2.5 mm | Feeler gauge |
| Blow-up ratio | 2.0–2.8:1 | Bubble diameter divided by die diameter |
| Frost-line height | 1–3 die diameters | Infrared pyrometer or visual scale |
| Melt temperature | 190–220 °C | Melt temperature probe |
| Specific energy input | 0.18–0.25 kW·h/kg | Extruder drive power divided by output |
| Hopper drying | Not normally required; if surface moisture is present, 60–70 °C for 2 h | Desiccant hopper dryer |
On a 90 mm single-screw extruder with 30:1 L/D, a barrier feed section, and a Maddock mixing section, D508A generally reaches throughput limits imposed by bubble cooling and melt fracture rather than by motor torque. With a 2.4 mm die gap and a 250 mm die diameter, the melt temperature window narrows to ±5 °C around 200 °C. At 195 °C, head pressure can run 10–20% higher than a 1.0 g/10 min LDPE-rich blend, and pressure transducer readings above 450 bar indicate that the screen pack or backpressure valve requires inspection. Specific energy input in the 0.18–0.25 kW·h/kg range is typical for LLDPE film extrusion; motors below 0.18 kW·h/kg may indicate low shear and poor mixing, while values above 0.25 kW·h/kg may indicate excessively tight screens or low temperatures.
Screw speed and output relationships are not linear in the low-melt-index LLDPE regime. As screw speed approaches 100 rpm on a 90 mm extruder, melt temperature rises due to shear heating; the increase can be 5–10 °C above the barrel set point. This limits the benefit of increasing screw speed and forces operators to adjust downstream cooling. Bubble cooling efficiency, expressed as specific airflow per kilogram of output, is usually more controlling than screw speed. Gauge is measured with a non-contacting capacitance or beta gauge; total thickness variation below ±5 µm is difficult to maintain if the die gap and air ring are not centered. When output is pushed beyond cooling capacity, frost-line height rises and bubble diameter oscillates with a period of 3–10 s.
Production floor failure modes include frost-line oscillation, gauge bands of ±5 µm from target, and bubble collapse at the nip during high ambient humidity. High-humidity collapse is managed by increasing stalk cooling airflow by 5–10% rather than by raising melt temperature alone; the bubble surface must remain below solidification temperature at the frost line. Persistent gauge bands require checking die-pin and die-lip eccentricity to within ±0.05 mm. Melt fracture on the bubble surface is usually controlled by raising die temperature by 5–10 °C or reducing output by 5–10%; if those measures are not acceptable, a fluoropolymer processing aid may be introduced at 200–800 ppm by weight, but the effect on printability and sealing should be evaluated. Quantitative output rates for this exact line configuration are not universally transferable; published data for this specific configuration is limited, and manufacturers should run trials.
Melt index alone does not define the processing behavior of D508A. The high-load melt index I₂₁ measured under ASTM D1238 at 190 °C/21.6 kg and the low-load melt index I₂ measured at 2.16 kg are used to calculate a flow ratio I₂₁/I₂; LLDPE grades in this melt-index class commonly fall between 15 and 20, but published data for this specific configuration is limited. Capillary rheometry at 190 °C and apparent shear rates of 100–400 s⁻¹ can show apparent viscosity of 300–500 Pa·s for a 0.5 g/10 min LLDPE; this value is not a specification but a guide for die-pressure prediction. The shear-thinning slope should be measured on the actual lot because comonomer distribution and molecular weight distribution influence extruder pressure more than the melt index value alone.
Heavy-duty sack qualification normally includes ASTM D1709 dart impact, ASTM D1922 Elmendorf tear, ASTM D882 tensile properties, and, when surface friction is specified, ASTM D1894 coefficient of friction. Comparative data should be generated at fixed gauge, typically 25 µm or 50 µm, and fixed blow-up ratio. Dart impact is highly gauge-sensitive; a 25 µm film can show a reduction of 50–80% relative to a 50 µm film on the same line, but the exact ratio is equipment-dependent. The optimum tear balance for D508A in monolayer film typically occurs between 2.2:1 and 2.6:1 blow-up ratio; outside this range, machine-direction and transverse-direction tear values diverge. When the film is tested after surface treatment, corona discharge can reduce ASTM D1894 coefficient of friction and increase wetting tension, but excessive treatment can oxidize the surface and reduce seal initiation performance.
In coextruded structures, D508A is often placed in the core layer at 40–60 wt% of total throughput, with LDPE skins. LDPE skins provide melt stability and seal initiation; D508A provides dart impact and tear resistance. Layer ratio optimization is line-specific and is usually evaluated against drop impact and seal strength rather than by melt index alone. For agricultural film, the base resin must be compounded with UV stabilizers; D508A is not supplied as a complete UV-stabilized compound unless specifically ordered. Without UV stabilization, service life is determined by accumulated solar irradiance and film thickness, not by an intrinsic property of the resin.
Compared with metallocene-catalyzed LLDPE film resins of similar density and melt index, D508A may show lower gloss and higher melt stability depending on molecular weight distribution and comonomer type; published data for this specific configuration is limited. Metallocene grades often produce higher clarity and lower extractables because of narrow composition distribution, but may require higher extruder torque and are more sensitive to screw wear. D508A is positioned for applications where film toughness and extrusion robustness carry more weight than optical clarity. Users selecting between D508A and metallocene LLDPE should compare ASTM D1003 haze, ASTM D2457 gloss, and ASTM D1922 tear at target gauge.
Food-contact status is established by the finished-article manufacturer under the intended conditions of use. As an olefin polymer, the base resin can be evaluated under 21 CFR 177.1520(c); however, the A suffix additive package may include slip and antiblock agents that require separate consideration. In the European Union, compliance is assessed under Regulation (EU) No 10/2011 after article-specific migration testing. The grade is not intended for medical implant applications. Pre-drying is normally unnecessary below 60% relative humidity; if surface condensation is observed, a desiccant hopper dryer at 60–70 °C for 2 h removes moisture. Sustained melt temperatures above 260 °C are not recommended because oxidative gel formation and odor risk increase. Standard polyethylene stabilizer packages are compatible; however, some color concentrates containing acid neutralizers or high-surface-area pigments can shift slip-agent migration and surface coefficient of friction. When ASTM D1894 coefficient of friction is a release specification, a conditioning period of 24–48 h after film production is commonly allowed for additive bloom.