| HS Code | 877619 |
| Product Name | Chevron Phillips 7109DT LLDPE Blown Film Resin, Hexene Copolymer |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Hexene-1 |
| Density | 0.918 g/cm³ |
| Melt Index 190 C 2 16 Kg | 0.7 g/10 min |
| Melting Point | 124 °C |
| Vicat Softening Point | 100 °C |
| Brittleness Temperature | -70 °C |
| Tensile Strength At Yield Md | 1400 psi |
| Tensile Strength At Break Md | 5000 psi |
| Tensile Strength At Break Td | 4500 psi |
| Elongation At Break Md | 600% |
| Elongation At Break Td | 700% |
| 1 Secant Modulus Md | 25000 psi |
| 1 Secant Modulus Td | 30000 psi |
| Elmendorf Tear Strength Md | 200 g |
| Elmendorf Tear Strength Td | 400 g |
| Dart Drop Impact F50 | 200 g |
| Haze | 12% |
| Gloss 45 | 60 |
| Coefficient Of Friction | 0.2 |
As an accredited Chevron Phillips 7109DT LLDPE Blown Film Resin, Hexene Copolymer factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Chevron Phillips 7109DT LLDPE Blown Film Resin, Hexene Copolymer is supplied in 25 kg (55 lb) polyethylene bags, palletized and shrink-wrapped. |
| Container Loading (20′ FCL) | 20′ FCL loaded with palletized 25 kg bags of Chevron Phillips 7109DT LLDPE Blown Film Resin, Hexene Copolymer, shrink-wrapped and secured. |
| Shipping | Chevron Phillips 7109DT LLDPE Blown Film Resin, Hexene Copolymer is shipped as non-hazardous solid resin pellets, typically in 25-kg bags or 1,000-kg bulk bags on pallets. Transport in clean, dry trucks or railcars. Keep away from moisture, heat, and direct sunlight. No special UN hazard classification is required. |
| Storage | Store Chevron Phillips 7109DT LLDPE Blown Film Resin, Hexene Copolymer in a cool, dry, well-ventilated warehouse. Keep original bags or containers sealed and palletized off the floor. Protect from direct sunlight, moisture, excessive heat, and ignition sources. Avoid dust accumulation and incompatible materials. Do not expose to open flames. Follow the manufacturer’s SDS and local regulations for safe storage. |
| Shelf Life | Chevron Phillips 7109DT LLDPE typically has a two-year shelf life when stored unopened below 50°C, away from sunlight and moisture. |
Primary-contact food packaging lines running Chevron Phillips 7109DT as a hexene-copolymer LLDPE typically operate monolayer blown-film extruders with 24:1–30:1 L/D barrier screws, a 1.5–2.5 mm die gap, and a melt temperature of 190–215 °C. The bubble is inflated at a blow-up ratio of 2.2–3.0 and collapsed through a Teflon nip with gauge variation held to ±5%; in-line corona treatment to 38–42 mN/m is specified before flexographic or rotogravure printing. The use of hexene comonomer rather than butene in the LLDPE backbone raises dart impact and Elmendorf tear when measured under ASTM D1709 and ASTM D1922, which permits downgauging of frozen food films without increasing puncture failures in vertical form-fill-seal machines. Incoming resin lots are checked for melt flow rate under ASTM D1238-20 at 190 °C/2.16 kg and density under ASTM D792-20 before release to extrusion.
For food-contact formulations, a representative blend is 65–85 wt% 7109DT with 15–35 wt% LDPE for bubble stability and melt strength, 2–4 wt% silica antiblock masterbatch, and 500–1000 ppm erucamide slip. The compounded film falls under FDA 21 CFR 177.1520(c) and EU Regulation (EU) No 10/2011, including the Annex V overall migration limit of 10 mg/dm². Terminal products manufactured from this configuration include pillow pouches for dry snacks, frozen food bags for IQF vegetables, bakery film for machine-twist closure, and light produce bags for loose leafy greens. The resin should not be specified for retort pouches or ovenable trays beyond 100 °C without separate migration and organoleptic testing.
Pinhole formation in heavy-duty industrial sacks is driven primarily by slow puncture under mass load and repeated flexing, not by tensile yield. Film converted from 7109DT at 100–180 µm is tested to ISO 7765-1:1988, ASTM D1709-15e1, ASTM D1922-09, and ASTM D882-18 before bag conversion. On a 90 mm grooved-feed extruder with 30:1 L/D, production-scale runs typically use a 2.5–3.0 mm die gap, a blow-up ratio of 3.5–4.5, internal bubble cooling, and a frost line height held at 25–40 cm. Bubble instability appears at high output when the collapse-frame approach angle drops below 20° or when the frost line is allowed to move more than ±5 cm, producing MD gauge bands and reduced dart impact at the edges. Melt temperature above 240 °C increases oxidative gel formation and must be avoided during extended stops.
Formulation for non-food heavy-duty sacks is commonly 100 wt% 7109DT for maximum puncture resistance, or 75–85 wt% with 15–25 wt% in-line edge trim regrind when bubble stability and die lines remain within specification. Black UV masterbatch is added at 2–4 wt% if the sacks are stored outdoors. For UN-certified dangerous goods sacks, the resin does not provide certification by itself; the converted sack must undergo the drop and stacking tests of the applicable packaging instruction and be marked with the UN specification code. Terminal types include liner bags inside woven polypropylene FIBCs, self-supporting rubble sacks for construction waste, and powder discharge liners for cement and mineral fillers.
In silage pit covers and greenhouse tunnel films, 7109DT is processed as the core or skin layer of 3-layer blown-film coextrusion lines with die diameters of 200–300 mm and layer ratios of 30/40/30 or 20/60/20. The die gap is typically 2.0–2.4 mm, the blow-up ratio 2.8–3.5, and the melt temperature 200–220 °C. Gauge control at ±6% is required for uniform UV additive distribution and to prevent early photodegradation at thin spots. The structure is collapsed, edge-slit, and wound on surface-center winders; anti-drip or antifog concentrates are dosed into the core layer only to limit bloom on the film surface. Field failures on agricultural lines are most often traced to uneven UV masterbatch distribution rather than base-resin mechanical loss.
Representative agricultural formulation: 60–75 wt% 7109DT, 15–25 wt% LDPE, 5–15 wt% EVA with 9–18% vinyl acetate, plus 0.2–0.8 wt% HALS, 0.1–0.3 wt% UV absorber, and 1–2 wt% anti-drip masterbatch. Compliance is assessed under EN 13206:2017 for agricultural covering films and, where relevant, the film must meet the national disposal and marking requirements under the EU Packaging and Packaging Waste Directive 94/62/EC. Finished articles include silage pit covers, greenhouse tunnel covers, low tunnels, and single-season mulching films. The resin without UV stabilization is not weatherable; outdoor service life cannot be predicted without accelerated weathering data referenced to ISO 4892-2 or EN 13206 exposure conditions.
The three-layer coextrusion route for opaque e-commerce mailers uses a core of post-consumer LLDPE recyclate between skins of 7109DT to preserve tear and seal performance while increasing recycled content. The layer ratio is commonly 20/60/20 with a total thickness of 50–80 µm; die gap is 2.0 mm, blow-up ratio 2.5–3.2, melt temperature 195–215 °C, and continuous screen changers with 150–250 µm screens protect the die from recyclate contaminants. Edge trim is re-pelletized in-line and returned to the core layer at up to 10–15 wt% without measured loss in machine-direction Elmendorf tear under ASTM D1922. Production bottlenecks include screen-pack plugging when post-consumer recyclate contains paper labels and melt fracture at the die lips when extruder barrel temperatures drop below 180 °C.
Representative formulation: 55–70 wt% 7109DT in the skin-plus-core matrix, 20–30 wt% post-consumer LLDPE recyclate, 10–15 wt% LDPE for bubble stability, and 3–5 wt% carbon black masterbatch. Because this application is non-food, regulatory compliance focuses on REACH Regulation (EC) No 1907/2006 and the EU Packaging and Packaging Waste Directive 94/62/EC, with heavy metals limits evaluated under 94/62/EC Article 11. Terminal products include opaque courier mailing bags, garment polybags, and protective void-fill pillow films. Incorporation of recyclate above 30 wt% may raise gel count and gauge variation; bubble cooling demand increases as melt strength drops.
At 25–50 µm, lamination sealant webs blown from 7109DT are specified for adhesive-laminated pouch structures where the sealant layer must deliver low seal initiation temperature, high puncture resistance, and acceptable clarity after lamination. The film is produced as a monolayer or coextruded web on a blown-film line with a die gap of 1.5–2.0 mm, blow-up ratio 2.0–2.8, melt temperature 190–210 °C, and corona treatment to 38–42 mN/m in line. It is then solventlessly laminated to BOPET, metallized PET, or aluminum foil at an adhesive coating weight of 2.0–3.5 g/m²; the laminate is cured at 40–50 °C for 24–48 h before slitting. Seal-strength testing is performed under ASTM F88/F88M-21, and the laminate is conditioned at 23 °C and 50% RH for at least 40 h before heat-seal measurement.
Formulation of the sealant web is 100 wt% 7109DT with 2–3 wt% antiblock masterbatch and 500–1000 ppm slip; for higher hot-tack requirements the addition of 10–20 wt% LDPE can lower seal initiation temperature but may reduce dart impact under ASTM D1709. Food-contact compliance is obtained under FDA 21 CFR 177.1520(c) and EU Regulation (EU) No 10/2011; the finished laminate must also account for the adhesive under FDA 21 CFR 175.105 or 21 CFR 175.300 if indirect contact is claimed. Terminal products include stand-up pouches for dry granular foods, frozen seafood pouches, and non-liquid sachets. The structure is not specified for retort or hot-fill above 95 °C because seal strength and laminate bond retention under thermal load require separate validation.
Competitive Chevron Phillips 7109DT LLDPE Blown Film Resin, Hexene Copolymer prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chevron Phillips 7109DT LLDPE blown film resin is a hexene-1-based linear low-density polyethylene supplied as pelletized resin. The nominal melt flow index is 0.90 g/10 min under 190°C/2.16 kg loading according to ASTM D1238, and the nominal density is 0.918 g/cm³ according to ASTM D1505. The product is distinct from butene-copolymer LLDPE grades of similar density because the hexene comonomer introduces longer short-chain branches during polymerization. In blown film, those longer branches alter the interlamellar tie-chain population, which is observed indirectly through dart drop resistance, Elmendorf tear, and slow crack-growth behaviour. Primary applications include heavy-duty sacks, industrial liners, frozen food packaging, and coextruded films requiring a balance of drawdown, bubble stability, and low-temperature puncture resistance.
Dart impact measurements under ASTM D1709 Method A do not describe an invariant resin property. The measured value is substantially modified by frost line height, die gap, internal bubble cooling, and deformation rate. On a 90 mm barrier-screw blown-film extruder with a 30:1 L/D, stable stalk formation at a blow-up ratio of 2.0–2.5 preserves the orientation balance that maintains dart impact. Too low a frost line leaves the film partially molten during expansion and can reduce transverse orientation; too high a frost line increases machine-direction orientation and reduces transverse-direction tear. For 7109DT at 25 µm nominal gauge, supplier-typical dart impact values near 210 g are obtained only within a narrow bubble-stability window. Deviation from the recommended die gap of 1.5–2.5 mm changes the effective draw ratio and can reduce the measured F50 value. The result is therefore a processing-dependent response, not a fixed resin specification.
Extrusion of 7109DT is generally run on single-screw extruders with L/D ratios from 24:1 to 30:1. Feed-throat temperatures near 180°C, compression-section temperatures of 200–215°C, and die temperatures of 215–225°C are typical; melt temperatures above 230°C can produce oxidative gels in high-shear zones. A barrier screw with a Maddock mixing element is used to complete melting, but excessively high shear can generate local overheating. Die pressure is controlled by the die land ratio; a land length ratio of 10:1 to 15:1 is common. A dual-lip air ring and internal bubble cooling are required above approximately 180 kg/h on a 300 mm die, although output limits depend on the line’s total heat-removal capacity. Pellets do not require pre-drying unless surface condensation is present; wet pellets introduced at the feed throat cause melt splay and local gel formation.
Typical supplier-published values for the resin and for 25 µm blown film are shown below. Values are not contractual specifications; they reflect a single film-production condition and will vary with additive package, die gap, and blow-up ratio.
| Property | Test method | Typical value |
|---|---|---|
| Melt flow index | ASTM D1238 | 0.90 g/10 min |
| Density | ASTM D1505 | 0.918 g/cm³ |
| Melting peak | ASTM D3418 | 124 °C |
| Vicat softening point | ASTM D1525 | 105 °C |
| Film gauge | — | 25 µm |
| Dart impact F50 | ASTM D1709 | 210 g |
| Elmendorf tear MD | ASTM D1922 | 340 gf |
| Elmendorf tear TD | ASTM D1922 | 450 gf |
| Tensile strength at break MD | ASTM D882 | 42 MPa |
| Tensile strength at break TD | ASTM D882 | 34 MPa |
| Elongation at break MD | ASTM D882 | 700 % |
| Elongation at break TD | ASTM D882 | 800 % |
| Haze | ASTM D1003 | 9 % |
| Gloss 45° | ASTM D2457 | 68 |
Lot-specific values should be obtained from the certificate of analysis because the additive package—especially slip, antiblock, and processing aid—affects haze, gloss, and coefficient of friction. Film optical properties also depend on melt temperature, frost line height, and air-ring turbulence; the same resin can produce a haze of 7–12% on different lines.
Differences from other products are significant when 7109DT is compared with butene-copolymer LLDPE, metallocene LLDPE, and high-pressure LDPE. Butene-copolymer LLDPE at 0.918 g/cm³ and 0.90 g/10 min may run with lower backpressure and can be lower in cost, but its dart impact and Elmendorf tear at equal gauge are generally lower because the butene branch is too short to generate the same load-bearing tie-chain concentration. Metallocene LLDPE grades have narrower molecular weight distribution, which improves dart impact and clarity but often reduces bubble stability and may require blending with 10–20% high-pressure LDPE. High-pressure LDPE contributes melt strength and bubble stability but reduces dart impact and tear at high loadings. 7109DT is positioned between conventional butene LLDPE and metallocene LLDPE: it provides higher toughness than many butene grades while retaining broader molecular weight processability.
In a three-layer coextrusion line, the core layer is run at 210–225°C while the skin layers may be held at 190–210°C to preserve seal initiation. A typical layer ratio is 20/60/20; raising the core fraction above 70% can raise die pressure and produce bubble instabilities on older air rings. High-pressure LDPE is often added at 10–20 wt% in the core to improve bubble stability; lower LDPE additions reduce gauge variation but do not fully replace internal bubble cooling. The use of 7109DT as the core in a 200 µm sack film improves drop-weight resistance relative to butene-copolymer core layers, although published data for this specific configuration is limited. When the structure is downgauged below 120 µm, the hexene copolymer’s tear balance becomes critical; transverse-direction tear typically decreases more than machine-direction tear as the film is drawn down.
Flow instabilities in single-screw extrusion are a common processing limit for LLDPE blown film. At low melt temperature, the resin exhibits high viscosity at the die lip, producing sharkskin or stick-slip melt fracture. Chrome-plated die lips with a land length of 15–20 times the die gap and melt temperature above 210°C reduce sharkskin. The use of polymer processing aids at 400–800 ppm may be required for high-output thin-gauge work; the DT grade may or may not include a processing aid, and the certificate of analysis should be checked. On a 90 mm extruder, backpressure is managed by adjusting the screen pack; a screen pack of 60/100/60 mesh can be used to trap contaminants but increases melt temperature at high throughput. Excessively high backpressure produces local overheating, gel counts, and die-lip buildup.
Elmendorf tear tests to ASTM D1922 and dart drop tests to ASTM D1709 are high-rate measurements; they rank film toughness but are not direct predictors of field puncture. A 25 µm film produced at a blow-up ratio of 2.0 may show machine-direction tear near 300 gf and transverse-direction tear near 500 gf, but increasing the blow-up ratio to 3.0 can invert the orientation balance and reduce transverse-direction tear. Because 7109DT is a hexene copolymer, the higher tie-chain concentration delays the onset of brittle failure in the dart test; film failures typically begin as ductile yielding rather than radial splitting. For routine quality assurance, both dart impact and Elmendorf tear should be collected after the line has reached steady state, because the first 30–60 minutes of production can show elevated haze and variable gauge due to thermal equilibration of the die and air ring.
Regulatory status: olefin polymers of this type are typically evaluated under FDA 21 CFR 177.1520 and European Union Regulation (EU) 10/2011; final food-contact suitability depends on migration testing at the intended thickness and temperature. The resin should not be used in continuous service above 80°C unless oxidative induction time and mechanical retention have been validated. Oxidative induction time is composition-dependent and should be specified for medical or electrical uses. Storage should be in a dry indoor environment below 50°C; extended storage beyond 12 months can shift slip-agent concentration at the film surface and alter coefficient-of-friction values. The material is combustible and must be processed with normal extrusion safety controls, including hopper magnet protection and screw cooling to avoid bridging in the feed zone.