| HS Code | 930292 |
| Density | 0.918 g/cm3 |
| Meltindex | 0.5 g/10 min (190°C/2.16 kg) |
| Tensilestrengthatyield | 1400 psi |
| Tensilestrengthatbreak | 3000 psi |
| Elongationatbreak | 800% |
| Flexuralmodulus | 30000 psi |
| Vicatsofteningpoint | 190°F |
| Brittlenesstemperature | < -100°F |
| Environmentalstresscrackresistance | > 1000 h |
| Dartdropimpact | 200 g |
| Elmendorftearstrengthmd | 250 g |
| Elmendorftearstrengthtd | 400 g |
| Haze | 12% |
| Gloss | 50 |
| Coefficientoffriction | 0.2 |
| Shoredhardness | 50 |
As an accredited Chevron Phillips 7105T LLDPE Sheeting Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 50 lb polyethylene bags, 40 bags per pallet (2,000 lb total) for Chevron Phillips 7105T LLDPE Sheeting Resin. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): Palletized 25 kg bags of Chevron Phillips 7105T LLDPE Sheeting Resin, stretch-wrapped, securely loaded for export. |
| Shipping | Chevron Phillips 7105T LLDPE Sheeting Resin is shipped as nonhazardous, solid polyethylene pellets. Standard packaging includes 25 kg bags, 1,000 kg bulk sacks, or bulk trucks/railcars, palletized and stretch-wrapped. Store dry, ventilated, away from heat and sunlight. Transport via truck or rail with no special DOT placarding or hazard class. |
| Storage | Store Chevron Phillips 7105T LLDPE Sheeting Resin indoors in a cool, dry, well-ventilated area, away from direct sunlight, heat, sparks, flames, and incompatible materials. Keep original containers sealed, labeled, and elevated on pallets. Avoid moisture, excessive stacking, UV exposure, impact, and contamination. Use first-in, first-out stock rotation. Ensure good housekeeping. Follow the manufacturer’s SDS and local regulations. |
| Shelf Life | Shelf life is typically 24 months when stored in original unopened packaging under cool, dry, well-ventilated conditions away from sunlight. |
Because oxygen ingress through a silage cover follows Fickian diffusion across the full film thickness, the use of a 150 µm blown monofilm from a butene-based LLDPE sheeting resin reduces gas transmission primarily by gauge rather than by base resin replacement. When 7105T is selected for this end use, the converter validates the finished film against EN 13207, which addresses thermoplastic silage films and tubes for agriculture; specimens are conditioned at 23 °C and 50 % RH before tensile and tear testing. The edge-fold zone is separately tested under ASTM D1922 Elmendorf tear because field failure propagates from clamp punctures, rodent damage, and wheel tears at the bunker shoulder. A blown-film line with a 2.0 mm die gap, a blow-up ratio of 2.2:1 to 2.8:1, and a melt temperature not exceeding 215 °C is used to balance machine-direction tear and transverse-direction dart impact; oxidative gel formation is controlled by keeping the melt residence time short and purging the die lips on a fixed interval. A HALS/UV absorber masterbatch is added at 1.0 % to 2.0 % by mass, with the let-down ratio verified through Xenon-arc exposure under ISO 4892-2 cycle 1 until the specified weathering retention is achieved. For a black-white coextruded cover at 200 µm, the white outer layer may contain 8 % to 12 % titanium dioxide by mass to reduce surface temperature and stabilise the stack against overheating. The terminal product is installed as a clamp cover or bunker sheet over ensiled maize, grass, or sorghum, with the film edges weighted by sandbags or soil and supplemented with a PE sealing tape at overlaps to interrupt the oxygen path at the clamped interface.
Processing consistency for silage sheeting is measured by film gauge profile, haze, and gel count rather than by melt index alone. On production-scale lines, the extruder screw typically uses a barrier mixer section with an L/D of 24:1 to 30:1; melt pressure before the screen pack is monitored because carbon black or TiO₂ masterbatch dispersion defects appear as gels that reduce dart impact under ASTM D1709. Film draw-down is controlled by a stable frost line height maintained between 6 and 8 times the die diameter, and collapsing-frame slats are inspected for burrs that cause longitudinal scoring. Field data from silage clamps show that failure at the clamp perimeter occurs earlier than failure of the central field area when the film is stretched beyond 10 % during installation; therefore, the supplier specification includes a maximum elongation at break under ISO 527-3 as a quality gate, not as a polymer selection parameter. REACH compliance for the compounded masterbatch must be confirmed because specific UV stabilisers and pigments migrate to the silage contact surface over time; extraction testing under EN 1186 may be required where the silage is subsequently used in food-producing animals.
In a 180 µm three-layer greenhouse covering produced from an LLDPE sheeting resin, the initial photosynthetically active radiation transmittance is measured with a quantum sensor and reported as a percentage of incident light, while haze is assessed under ASTM D1003 and total light transmittance under ISO 13468-1. The outer layer is compounded with a UV stabilizer package so that the film retains at least 50 % of its original tensile elongation after 8,000 hours of Xenon-arc exposure under ISO 4892-2; the inner layer contains an anti-fogging additive that migrates to the surface over 24–48 hours and reduces discrete droplet condensation. If the anti-fog additive is overdosed, surface bloom creates a tacky layer that attracts dust and lowers PAR transmittance by 5–10 % over one season. The middle layer may contain EVA at up to 10–15 % by mass to increase light diffusion and low-temperature impact strength, but raising EVA content above this range reduces bubble stability on a conventional low-pressure die. The film is extruded on a blown-film line with a blow-up ratio of 2.5:1 to 3.0:1, a die gap of 1.8 mm to 2.1 mm, and a melt temperature of 190 °C to 210 °C. The terminal greenhouse cladding must be installed with the anti-fog-treated surface facing inward; installation tension must remain below 2 % elongation to avoid reducing the mechanical anchorage at the clamp profile.
Surface roughening caused by soil abrasion and UV exposure changes the wetting angle of the inner surface, which is why greenhouse films are assessed for contact angle and haze development after weathering rather than only for initial transmission. A production-scale bubble collapses through a wooden or PTFE collapsing frame; PTFE slats reduce surface scratching of the hot tube, which is critical for retaining optical uniformity. The winding tension is maintained between 10 and 15 N/m to prevent blocking while avoiding stretched rolls that distort the gauge profile. For a multi-season cover, the specification may require a minimum dart impact value under ASTM D1709 and a minimum Elmendorf tear value under ASTM D1922 because hail and sharp greenhouse frame points are the primary puncture sources. The final product is cut into tunnel covers, gable-end bodies, or side-roll curtains; seam welding is conducted with hot air or impulse welders that operate at 120–150 °C on the LLDPE surface, and the weld strength is checked according to EN 12814-4 for thermoplastic welds. Without stabiliser verification under EN 13206, a greenhouse film supplied with indoor-grade LLDPE would fail after one season, so the converter must hold a batch-specific weathering certificate for the UV package used in 7105T.
ASTM C171 establishes the moisture retention limits for sheet-form concrete curing covers, and a 0.10 mm to 0.15 mm LLDPE sheeting film is placed over fresh concrete within 24 hours of finishing to reduce evaporative water loss. The water vapour transmission rate is measured at 38 °C and 90 % RH according to ASTM E96/E96M; a black-pigmented film used for heat retention commonly contains 2 % to 4 % carbon black by mass. Dispersion quality is checked by screen pack pressure rise on the film line; a pressure increase greater than 20 bar over 8 hours indicates poor masterbatch distribution and predicts reduced film tear resistance. The cover is produced on a cast film line with a polished chill roll at 20–30 °C, which creates the flat surface needed for overlap taping and prevents the film from curling at the slab edges. On large slab pours, film sheets are overlapped by 300 mm to 500 mm and continuously taped or covered with a sand load to maintain contact with the concrete; wet subgrade installations require a film with a broader width tolerance because soil particles under the sheet cause localised puncture under foot traffic.
Field data from concrete curing installations show that the highest moisture loss occurs at the slab edge and at column penetrations, where the membrane is cut and reattached. A cured concrete slab covered by an LLDPE sheet retains a higher surface moisture content than an uncovered slab for the first 7 days, but the film must be removed for saw cutting and then resealed. The concrete curing membrane’s tensile properties are evaluated under ISO 527-3 after outdoor exposure to ensure that UV-induced embrittlement does not cause failure during extended construction delays; when a weathering requirement is absent, film exposed for more than 30 days should be replaced before final dry-in. Because concrete alkalinity can react with certain stabiliser systems, the converter confirms that the masterbatch formulation is compatible with high-pH drainage water and does not contribute to staining of light-coloured architectural concrete; extraction behaviour may be checked under EN 1186 when the concrete surface is subsequently used for potable water contact. The terminal product is cut to slab dimensions on site and reused only if it passes a visual inspection for abrasion and punctures.
The question is resolved by specifying the finished geomembrane under GRI-GM17, which applies to LLDPE geomembranes and includes minimum thickness, carbon black dispersion, and oxidative induction time requirements. A 1.0 mm or 1.5 mm sheet produced from an LLDPE sheeting resin by flat-die extrusion or calendering is tested for tensile properties under ASTM D6693, puncture resistance under ASTM D4833, and tear resistance under ASTM D1004. The polymer melt is processed at 230 °C to 260 °C through a slot die with a polished roll stack; the roll gap is set to the final sheet thickness plus 0.05 mm to 0.10 mm of compression allowance, and the line speed is controlled to maintain a thickness tolerance of ±10 %. In landfill drainage applications, the geomembrane is installed over a geocomposite drain and covered with a protection geotextile; the site engineer accepts the LLDPE sheet only when seam peel adhesion tested under ASTM D6392 meets the project’s specified minimum in both shear and peel mode. The wedge welder operates at 400–450 °C, and the overlap width is maintained at 75 mm to 100 mm to allow a weld track with air channel testing.
LLDPE geomembranes made from sheeting resin provide greater flexibility and multiaxial elongation than HDPE geomembranes, which makes them suited for detailed slopes and stack closures, but the puncture resistance at equivalent thickness is lower; therefore, a 1.5 mm LLDPE sheet may be specified where a 1.0 mm HDPE sheet would otherwise be accepted. The installer verifies carbon black dispersion by microscopic examination under GRI-GM17 because low dispersion creates stress concentrations that reduce stress crack resistance. Oxidative induction time is measured under ASTM D3895 at 200 °C; the specification value is set by the design engineer and depends on the service temperature and the aggressiveness of the retained liquid. For a heap leach pad or secondary containment basin, the liner must be tested for resistance to the specific chemical solution at the maximum operating temperature; published data for 7105T in this specific configuration is limited, so an immersion test under ASTM D5747 is recommended before final specification. Field installation on slopes above 3H:1V uses additional anchor trenches and geotextile cushioning, and the LLDPE sheet is not walked on with cleated boots until a geotextile protection layer has been placed over it.
| End use | Critical property | Test standard | Conditioning or apparatus |
|---|---|---|---|
| Silage barrier film | Tensile retention after weathering | EN 13207 | Xenon-arc under ISO 4892-2 cycle 1 |
| Greenhouse cladding | Haze and PAR transmittance | ASTM D1003 / ISO 13468-1 | 23 °C, 50 % RH; quantum sensor |
| Concrete curing membrane | Water vapour transmission rate | ASTM E96/E96M | 38 °C, 90 % RH, desiccant method |
| LLDPE geomembrane | Puncture resistance | ASTM D4833 | 23 °C, 50 % RH, clamped specimen |
| Heavy-duty sack liner | Seal peel strength | ASTM F88/F88M | 23 °C, 50 % RH, 300 mm/min jaw speed |
For heavy-duty industrial sacks used in mineral and chemical packaging, an LLDPE sheeting resin is converted into a 60 µm to 100 µm inner film that is either inserted as a loose liner or laminated to a woven polypropylene outer ply. The film is produced on a blown-film line equipped with a grooved-feed extruder, a 2.0 mm die gap, and a blow-up ratio of 2.0:1 to 2.5:1; the resulting bubble has a low stalk height to maintain impact toughness. Seal integrity is evaluated by the bag drop test under ISO 7965-2, and the weld is tested by tensile-peel under ASTM F88/F88M after the film is converted on a bottom-seal or side-seal bag line. The resin’s melt strength is insufficient for very tall vertical bag lines unless the die gap is opened and the melt temperature is lowered to 185 °C to 200 °C; this reduces melt draw-down and permits stable bubble formation at large diameters. Slip and antiblock additives are incorporated at 500 ppm to 1,000 ppm by mass to prevent blocking of the film rolls during high-humidity storage; the exact addition level is set by the coefficient of friction target, which is measured under ISO 8295.
The terminal sack is filled with product at 25 kg to 50 kg per unit and drop-tested from 1.2 m; failures occur predominantly at the film weld, so process control on the bag line is limited to a seal temperature window of ±5 °C for LLDPE grades. If the LLDPE inner film is used as a moisture barrier in a paper-plastic multi-wall sack, the ply is laminated with an EVA or LDPE tie layer at 5–8 g/m²; the laminated structure is checked for bond strength under ASTM D903 to prevent delamination during filling. For products requiring food-contact compliance, the film formulation is assessed under FDA 21 CFR 177.1520 and the colour masterbatch supplier must provide a Directive 10/2011/EU migration certificate. The converter must also verify that the film does not pinhole at folds or gusset points; pinhole inspection is performed with a light table or corona-treated film with a wetting tension above 38 mN/m to ensure print adhesion on the outer ply.
Competitive Chevron Phillips 7105T LLDPE Sheeting Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chevron Phillips Chemical 7105T is a linear low density polyethylene sheeting resin supplied for cast sheet and heavy-gauge sheet extrusion where low-temperature toughness, moderate rigidity, and deep-draw thermoforming are required together. The grade is characterized by a nominal density of 0.918 g/cm³ determined under ASTM D1505 and a melt index of 0.50 g/10 min measured at 190°C and 2.16 kg using ASTM D1238 or the equivalent ISO 1133-1:2022 method. These two specification anchors place 7105T in the conventional high-molecular-weight LLDPE sheet segment, separate from branched low-density polyethylene and from high-density or metallocene-based sheet resins. The linear backbone with short-chain branching provides higher tensile strength and puncture resistance than a branched LDPE of similar melt index, while the melt strength is lower than that of LDPE and must be addressed through die-to-roll geometry. The product is supplied as pelletized material and is processed on conventional single-screw lines with barrier screws; however, lot-specific certificates of analysis should be consulted for acceptance criteria.
Table 1. Core grade-characterization parameters.
| Parameter | Typical value | Standard or source |
|---|---|---|
| Density | 0.918 g/cm³ | ASTM D1505 |
| Melt index | 0.50 g/10 min | ASTM D1238 |
| Melt index equivalent | 0.50 g/10 min | ISO 1133-1:2022 |
| Supply form | Pellets | Supplier specification |
The combination of density and melt index does not by itself define fitness for a specific sheet application. Density influences stiffness, barrier, and heat resistance, while melt index reflects only a low-shear viscosity point at 190°C; it does not capture the entire shear-thinning curve, extensional viscosity, or melt strength that govern sag and draw behavior. For 7105T, the 0.918 g/cm³ density supports a balance between toughness and stiffness, while the 0.50 g/10 min melt index is selected to provide sufficient melt strength and mechanical integrity for heavy-gauge sheet. Processors should not use melt index as a direct predictor of extrusion motor load, because LLDPE resins with the same melt index as LDPE typically require more torque at production shear rates.
Relative to branched LDPE at the same nominal melt index, 7105T exhibits higher shear viscosity in the low-shear region and a more gradual shear-thinning response under typical extrusion conditions. Production-scale single-screw lines therefore record higher melt pressure and motor load when converting from an LDPE of comparable 0.50 g/10 min melt index at the same screw speed and barrel profile. In sheet extrusion, this viscosity difference is managed by increasing torque capacity and by using barrier screws with 24:1 to 30:1 L/D ratios rather than by relying on excessive melt temperature. Compared with metallocene LLDPE grades designed for film clarity or hot-tack, 7105T is positioned for heavy-gauge sheet and thermoforming, not for blown film. The supplier’s published data may not identify the specific comonomer type; many conventional LLDPE sheet resins in this density range are butene copolymer grades, but comonomer identity should be confirmed through the supplier technical data sheet. In downstream handling, the grade does not require the extremely tight die-gap control sometimes specified for metallocene resins; the principal operational constraint is the lower melt strength of linear polyethylene, which increases neck-in and draw resonance if draw-down ratio or die-to-roll distance is excessive.
Compared with high-density polyethylene sheet of similar melt index, 7105T delivers lower flexural modulus and higher low-temperature impact resistance, but it also has a lower continuous-use temperature and lower crush resistance. This distinction is relevant for packaging, agricultural, and industrial sheet applications that demand puncture resistance and deep-draw capability rather than high stacking strength. In multi-layer constructions, HDPE may be preferred for core stiffness while 7105T is selected for the outer ply. The selection between LLDPE and HDPE is therefore made from the part’s required modulus, impact resistance, and thermoforming draw ratio rather than from melt index alone.
On monolayer chill-roll sheet lines, 7105T is extruded through a single-screw machine with a barrier or Maddock mixing section. Barrel setpoints between 190°C and 230°C are typical, with adapter and die zones maintained from 200°C to 240°C. Melt temperature should be measured at the adapter because barrel setpoints alone do not account for shear heating. Extended residence time above 260°C can generate oxidized gel particles and yellowing in unpigmented thin-gauge sheet. A starting die gap of 0.5 mm to 1.0 mm is used for sheet thicknesses between 0.25 mm and 1.5 mm, with final gauge set by chill-roll speed and nip pressure. Chill-roll temperatures of 20°C to 40°C are adopted to balance crystallinity, surface replication, and sheet flatness. Because LLDPE has lower melt strength than LDPE, the die-to-roll gap is minimized to reduce neck-in. Edge trim from unpigmented sheet is recycled as regrind only after moisture and incompatible polymer contamination are controlled.
Melt-pressure instability at the die is a recognized bottleneck when 7105T is processed on lines designed for LDPE. Head pressure may exceed the die design limit if screw speed is increased without corresponding die-temperature adjustment. Surface defects classified as sharkskin can appear under high die shear stress; the use of a fluoroelastomer-based polymer processing aid at 200 ppm to 800 ppm may condition the die surface and delay melt fracture. Conditioning should follow the processing-aid supplier’s schedule, since rapid rate increases before full die coverage may produce temporary haze or surface roughness. Extruder drive capacity is checked before production, because viscosity-limited torque may restrict output before the thermal degradation boundary is reached.
Melt strength of 7105T is inherently lower than that of branched LDPE because the linear architecture lacks long-chain branching. The practical consequence is that a sheet line designed for LDPE may require a shorter draw distance, a wider die with edge bead, or a higher nip entry angle. At elevated line speeds, the web may exhibit draw resonance, a periodic thickness variation along the machine direction, if the stretch ratio exceeds a critical value. The threshold depends on die gap, melt temperature, and draw distance; it is not an intrinsic resin property that can be stated without line-specific data. Processing aids and melt temperature adjustments can shift the onset of draw resonance only within a narrow range, so mechanical configuration changes are usually required.
Sheet produced from 7105T develops a crystallinity gradient through the thickness because the chill-roll surface cools the web faster than the core. This gradient influences thermoforming draw uniformity, trim shrinkage, and impact resistance. In production, roll-stack temperature is stabilized to maintain consistent surface gloss and to avoid differential shrinkage that appears as edge curl or wave distortion. Thermoforming operations typically heat the sheet to a surface temperature below the Vicat softening range but high enough to permit sag control; actual settings depend on sheet thickness, heating power, and part geometry. The grade’s high molecular weight tail contributes to melt strength during plug-assisted forming, but published data for the specific sag limits of 7105T are limited, so forming trials should establish the heating schedule and plug temperature for each mold.
Mechanical acceptance testing of 7105T sheet is usually performed according to ASTM D638 for tensile properties at 50 mm/min and ASTM D3763 for high-speed puncture resistance. Low-temperature impact is assessed with instrumented puncture after conditioning at -18°C or by the end-user’s part-level drop test. The exact acceptance values are part-specific and are not supplied by the resin property table alone. A lot that meets density and melt index specifications can still fail a thermoformed part test if sheet thickness distribution, regrind history, or heat exposure differs from the qualification lot. Therefore, incoming resin inspection is supplemented by retained sheet samples and by monitoring extruder melt pressure, melt temperature, and chill-roll temperature against the qualified operating window.
7105T may be coextruded as a skin layer over high-density polyethylene, polypropylene, or regrind core layers to provide toughness and sealing characteristics while retaining the core layer’s stiffness or cost structure. Coextrusion requires separate extruders with dedicated melt-temperature control, and the skin-layer extruder is sized for the desired layer ratio. Melt-phase adhesion between the LLDPE skin and an HDPE or regrind core is typically sufficient for many sheet applications, but incompatible tie-layer chemistry may be required if the core is polypropylene or an EVOH barrier layer. Die design for the multi-layer structure should account for the different viscosity ratios of the skin and core; an apparent viscosity ratio departing from approximately 1:1 at the die shear rate can encourage interfacial instability, visible as internal waviness or transfer of surface defects. Sheet converters often maintain the edge-trim layer ratio and reintroduce mixed regrind into the core layer only, preventing skin-layer contamination by degraded polymer. On production lines, layer distribution is monitored by thickness measurement after each chill roll and by destructive cross-sectional analysis under optical microscopy.
Edge-trim handling for 7105T requires separation by layer type in coextruded structures. Mixed regrind containing polypropylene or EVOH creates incompatible domains that can reduce impact strength and produce surface gels if blended into the LLDPE skin. Regrind ratio limits are typically established by measuring extruder filtration pressure and visual defect counts on finished sheet; a filter pack with 100 µm to 200 µm mesh is used on many sheet lines to remove char and agglomerated contaminants. Regrind moisture content should remain below 0.05 wt% before reintroduction, because trapped volatiles can create pinholes in thin-gauge sheet. These operational limits are line-specific and should be fixed through trial data rather than transferred from dissimilar equipment.
For 7105T, predrying is generally not required when pellets are stored in sealed containers and ambient relative humidity remains below 60%. If surface moisture is observed or if regrind has been exposed to condensation, drying at 60°C to 80°C for 2 h to 4 h with a desiccant dryer is a conservative starting point; however, published data for the specific water pick-up of 7105T are limited. Purge protocols should use a purging compound or a high-viscosity polyethylene to remove residual LLDPE from the barrel before long shutdowns, because prolonged residence time at melt temperature can generate carbonized deposits. The resin should not be combined with amine-based additives that can promote discoloration or with certain peroxide masterbatches intended for crosslinking, because uncontrolled chain modification may shift rheology and gel content. Ultraviolet stabilization for outdoor sheet is achieved through a suitable hindered-amine light stabilizer and UV absorber package, but the choice should be qualified by weathering tests such as ASTM G154 or ISO 4892-2:2013 on the finished sheet rather than on pelletized resin alone.
Table 2. Regulatory reference matrix for end-use qualification.
| Framework | Reference | Verification requirement |
|---|---|---|
| United States food contact | 21 CFR 177.1520(c) | Obtain supplier compliance letter for end-use conditions |
| European Union food contact | Regulation (EU) No 10/2011 | Obtain Declaration of Compliance with migration limits |
| REACH | EC 1907/2006 | Verify SDS Section 15 and SVHC status |
| RoHS | Directive 2011/65/EU | Supplier declaration for electrical and electronic applications |
In heavy-gauge thermoforming, 7105T sheet is heated to a surface temperature typically between 125°C and 160°C, measured with an infrared pyrometer, rather than by oven setpoint alone. The high molecular weight tail resists corner and sidewall thinning during plug-assisted forming, but excess heating causes sag and web distortion. Formed parts are conditioned at -18°C and 23°C before impact testing to verify low-temperature toughness under end-use conditions. Because published data for the specific sag limits of 7105T are limited, mold-specific heating profiles and plug-temperature settings are established through production trials and retained with batch records.