| HS Code | 549733 |
| Density | 0.918 g/cm³ |
| Melt Mass Flow Rate Mfr | 50 g/10 min |
| Tensile Strength At Yield | 10.3 MPa |
| Tensile Strength At Break | 12.4 MPa |
| Elongation At Break | 500% |
| Flexural Modulus | 0.234 GPa |
| Shore D Hardness | 50 |
| Melting Point | 122 °C |
| Vicat Softening Temperature | 93 °C |
| Deflection Temperature At 0 46 Mpa | 43 °C |
As an accredited Chase Plastics CP Pryme® PE100LLD-50M Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 50 lb multiwall bags, palletized and stretch-wrapped for secure shipping and storage. |
| Container Loading (20′ FCL) | 20′ FCL loaded with palletized 25 kg bags of Chase Plastics CP Pryme PE100LLD-50M LLDPE, shrink-wrapped and secured for transport. |
| Shipping | Chase Plastics CP Pryme® PE100LLD-50M is a non-hazardous linear low-density polyethylene, usually shipped as pellets in 50 lb bags, bulk bags, or bulk containers. Transport in clean, dry, covered vehicles at ambient temperature; avoid moisture, heat, UV, and contamination. Not regulated by DOT/IMDG/IATA; consult SDS. |
| Storage | Store Chase Plastics CP Pryme® PE100LLD-50M in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, ignition sources, and strong oxidizers. Keep original containers or bags closed, labeled, and off the floor on pallets. Prevent moisture, dust, and physical damage. Maintain stable ambient temperature and avoid prolonged UV exposure. Follow local regulations and SDS recommendations. |
| Shelf Life | Stable under recommended storage; no specific shelf life. Keep cool, dry, sealed, and protected from UV light, heat, and contaminants. |
Where rotationally moulded agricultural chemical storage represents the highest-volume downstream use, the processing sequence begins with dry blending rather than melt compounding. Chase Plastics CP Pryme® PE100LLD-50M Linear Low Density Polyethylene is charged at 85 wt% virgin powder, 15 wt% clean in-house rotomoulding regrind of identical chemistry, and 2.0 wt% of a PE-carrier UV masterbatch containing 8 wt% hindered amine light stabilizer. The applicable minimum design standard is ASTM D1998-21 for upright polyethylene storage tanks, while long-term stress-cracking acceptance is referenced to ASTM D1693-15 condition B because surfactant-based pesticide and foliar fertilizer formulations attack microscopic melt-fusion boundaries above the liquid line. Characteristic technical data sheet values used in downstream process setting include a nominal melt flow rate of 5.0 g/10 min at 190°C/2.16 kg under ASTM D1238 and a nominal density of 0.935 g/cm³ under ASTM D1505. In a four-arm carousel oven with an aluminium mould, the powder is sintered at 280–300°C for 22–26 min; primary-axis rotation at 8 min−1 and secondary-axis rotation at 2 min−1 produce a 4:1 ratio that holds wall thickness between 4.5 mm and 8.0 mm along vertical baffle seams. Cooling starts with forced air at 0.8–1.2 m/s until the part surface falls below 105°C, after which fog mist is introduced to prevent warpage at fitting inserts. When warehouse relative humidity exceeds 60%, the powder is pre-conditioned at 60°C for 1 h because surface moisture expands during the oven plateau and forms pinholes at the thinnest wall section. Terminal parts are above-ground fertilizer mixing tanks, chemical dosing tanks, and secondary containment basins of 2,000–35,000 L capacity. The dominant production rejection is pinhole formation when oven setpoint falls below 260°C or when regrind exceeds 20 wt%, because residual thermal history at particle boundaries cannot be fully healed under normal carousel residence time.
| Application sector | Primary standard or regulation | Typical oven setpoint | Wall thickness | Formulation addition ratio |
|---|---|---|---|---|
| Agricultural storage tanks | ASTM D1998-21, ASTM D1693-15 | 280–300°C | 4.5–8.0 mm | 85 wt% virgin, 15 wt% regrind, 2.0 wt% UV masterbatch |
| Chemical feed tanks | ASTM D1998-21, NSF/ANSI 61 where certified | 265–285°C | 4.0–7.5 mm | ≤10 wt% regrind, 1.5 wt% carbon black-HALS masterbatch |
| Kayak hulls | ISO 12217-1:2015 | 270–285°C | 4.5–6.0 mm | 95 wt% virgin, 5 wt% regrind, 2.0 wt% colour masterbatch |
| Marine floats | 33 CFR 183.114 | 275–290°C | 6.0–8.0 mm | 100 wt% shell, PU foam 60±5 kg/m³ |
| Playground components | ASTM F1487-21, EN 1176-1:2017 | 275–290°C | 5.0–6.0 mm | 95 wt% virgin, 3.0 wt% colour, 2.0 wt% UV/HALS |
| Insulated cooler liners | FDA 21 CFR 177.1520 | 270–280°C | 3.0–5.0 mm | 100 wt% virgin liner, PU foam 40–50 kg/m³ |
| Material handling hoppers | 49 CFR 178.509 where UN-certified | 280–290°C | 5.0–9.0 mm | 98.5 wt% virgin, 1.5 wt% antistatic masterbatch |
Chemical feed tanks for water treatment require a lower oven temperature than agricultural storage to preserve flatness of double-wall containment floors. The powder is charged at 100 wt% virgin CP Pryme® PE100LLD-50M with 1.5 wt% carbon black-HALS masterbatch; closed-loop regrind is held at or below 10 wt% because sodium hypochlorite and polyaluminium chloride generate stress cracking preferentially at regrind particle boundaries. The design baseline remains ASTM D1998-21, and potable water contact is permitted only where the moulded tank and the specific powder lot are certified to NSF/ANSI 61; uncertified parts are restricted to non-potable chemical dosing, sewerage, and rainwater reuse. Processing in a fabricated steel mould uses an oven setpoint of 265–285°C and internal air pressure of 35–60 kPa during the final 6 min of heating to press the inner wall against the mould and reduce void formation at threaded boss lands. Wall thickness below 4.0 mm is not recommended for sodium hypochlorite service because local hoop stress near the lower sidewall under 500 mm liquid head can exceed the long-term environmental stress-cracking threshold after 8,000 h of intermittent exposure. Demoulding is performed only after the part cools to 60°C; premature demoulding produces sink marks at integrally moulded baffle plates. Terminal parts are 200–5,000 L day tanks, double-wall containment basins, and chemical feed skid enclosures. The operational boundary for high-alkaline or oxidising mixtures is that published immersion data for this specific moulded configuration remains limited, so tank qualification at the specified wall thickness is required before long-term service.
Kayak hull production uses the narrowest sieve distribution of the powder because the exterior surface must not show pinholes along the keel radius, particularly where later mechanical fasteners penetrate the hull. The formulation is 95 wt% virgin powder, 5 wt% clean regrind from trimmed hatch openings, and 2.0 wt% high-opacity colour masterbatch; no inorganic filler is added because filler raises flexural modulus and shifts the ductile-to-brittle transition toward cold-water service temperature. Compliance for the complete small craft is assessed under ISO 12217-1:2015, and where closed-cell buoyancy foam is introduced into sealed compartments, 33 CFR 183.114 flotation material acceptance applies. The clamshell mould is closed under 0.6–0.8 MPa clamping force and rotated biaxially in an oven at 270–285°C for 18–25 min, followed by forced-air cooling to 110°C and then water mist to suppress sink marks at scupper and seat-retainer inserts. Demoulding occurs at 55°C. Terminal parts are rotomoulded sit-on-top and sit-inside kayak hulls of 3.5–4.9 m length, with wall thickness measured between 4.5 mm and 6.0 mm; the primary scrappage defect is void formation at the hull-to-deck bonding flange when oven residence time is shortened by more than 15%. Rapid water-quench cooling below 50°C at demoulding is avoided because residual stress around the deeply drafted bow inserts later releases as stress whitening under hull impact.
For floating walkways and dock floats, the moulded shell functions more as a buoyancy envelope than a structural hull, so acceptance shifts toward flotation material retention and foam stability. The outer shell is charged as 100 wt% CP Pryme® PE100LLD-50M with 2.0 wt% UV/HALS masterbatch; no regrind is used in the water-facing exterior because seawater extraction of degraded particle boundaries is a known long-term failure mechanism in tidal mooring systems. The shell is rotationally moulded at 275–290°C to a wall thickness of 6.0–8.0 mm, then drilled for vent ports before a two-component polyurethane foam system with density 60±5 kg/m³ is injected. The foam is evaluated for water absorption under ASTM D2842, and where the float forms part of a moored small craft buoyancy system, 33 CFR 183.114 applies to the cellular plastic foam. The critical process conflict is exothermic cavity pressure during foam rise, which can deform the shell if vent scheduling is not matched to the formulation gel time; published correlation data for cavity pressure at this wall thickness remains limited, so mould trials with cavity pressure sensors are required to set the vent schedule. Terminal parts are hexagonal dock floats, pontoon buoyancy blocks, and aquaculture raft shells, often with integrally moulded chain bosses where insert torque is limited by the insert supplier to prevent stress cracking in the LLDPE wall.
Because playground structural components are exposed to outdoor weathering, the dry blend is formulated with a higher colour-masterbatch loading than agricultural parts. The blend is 95 wt% CP Pryme® PE100LLD-50M, 3.0 wt% colour masterbatch, and 2.0 wt% UV/HALS stabilizer; post-consumer regrind is excluded from visible surfaces to maintain the impact and entrapment requirements of ASTM F1487-21 and the European equivalent EN 1176-1:2017. In a three-arm carousel, the mould is rotated at a 4:1 ratio in a 275–290°C oven for 20–24 min, producing a wall thickness of 5.0–6.0 mm for tunnel sections, slide hoods, and climbing pods; after demoulding at 60°C, components are trimmed and checked for internal wall separation at sharp radii using an ultrasonic thickness gauge. The main process limitation is that increasing wall thickness above 6.5 mm extends cycle time without proportional structural benefit and increases warpage when cooling rate is non-uniform across the mould.
Insulated coolers made from rotationally moulded LLDPE use a two-part or multi-charge process because the inner food-contact liner and exterior shell are joined around a polyurethane foam core. The inner liner formulation is 100 wt% virgin CP Pryme® PE100LLD-50M, with no regrind unless the regrind has been generated solely from approved food-contact lots and is covered by FDA 21 CFR 177.1520 conditions for olefin polymers; the exterior shell may contain 2.0 wt% UV/HALS masterbatch. The liner is processed at 270–280°C with wall thickness between 3.0 mm and 5.0 mm, followed by injection of rigid polyurethane foam with density 40–50 kg/m³ between the shells. Because polyethylene has low surface energy, chemical adhesion to the foam is unreliable, so mechanical interlock through integrally moulded ribs or drilled microperforations is required. Terminal parts are 30–120 L insulated ice chests, fish boxes, and controlled-temperature transport containers; the food-contact claim applies only to the virgin inner liner and does not automatically extend to the recycled exterior shell. The main operational limitation is that closed-cell foam expansion can distort a liner thinner than 3.0 mm, so minimum wall thickness is maintained at the bottom radius where foam injection pressure peaks.
Because material handling hoppers and pallet bins are designed for cold impact and fork-tine abrasion, the processing parameters prioritise wall thickness over short cycle time. The blend is 98.5 wt% virgin powder and 1.5 wt% antistatic masterbatch where electrostatic discharge control is specified; regrind may be added up to 20 wt% for non-certified surfaces, but UN-certified plastic drums and jerricans used for hazardous liquid transport must satisfy 49 CFR 178.509 drop and hydrostatic test requirements with the intended regrind ratio. Oven setpoint is 280–290°C for 24–30 min in steel moulds with internal gussets, yielding wall thickness from 5.0 mm to 9.0 mm at fork pockets. Terminal parts include 0.5–2.2 m³ hoppers, fish totes, and general industrial pallet bins. The main process limitation is that water-quench cooling below 50°C after demoulding can introduce residual stress at internal corners, which later releases as stress whitening under impact at −20°C.
Competitive Chase Plastics CP Pryme® PE100LLD-50M Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chase Plastics CP Pryme® PE100LLD-50M Linear Low Density Polyethylene is a high-melt-flow LLDPE grade positioned for processing routes where low melt viscosity is the primary determinant of manufacturability: thin-wall injection molding, cast film and extrusion coating, high-speed compounding, and masterbatch carrier systems. The material is identified by melt mass-flow rate under ASTM D1238-20 or ISO 1133-1:2022 at 190 °C with a 2.16 kg load; the nominal class is 50 g/10 min, while the exact lot value and density are listed on Chase Plastics’ certificate of analysis. Density, when measured by ASTM D792-20 or ISO 1183-1:2019, falls within the commercial LLDPE range of 0.915–0.940 g/cm³ for high-flow copolymers, but the specific value must be confirmed from lot documentation because comonomer type and polymerization conditions shift density within that range.
The product is differentiated from 20-MFI general-purpose LLDPE primarily by lower average molecular weight and reduced chain entanglement. That molecular difference lowers shear viscosity and improves flow length in a mold, but it also reduces slow-crack-growth resistance and environmental stress-crack resistance. The 50 melt-flow designation should therefore be treated first as a processing parameter and second as a durability proxy.
In injection molding, the low melt viscosity supports wall thicknesses down to 0.30 mm on machines with clamp forces from 800 kN to 3,000 kN. Typical barrel temperature profiles range from 180 °C at the feed throat to 230 °C at the nozzle, with mold temperatures held between 10 °C and 40 °C. Injection speed should be set to high velocity on thin-wall parts to avoid premature freeze-off; however, shear rates beyond approximately 40,000 s−1 can introduce melt fracture or gate blush in hot-runner systems with restricted gate diameters. The material does not require routine drying at ambient humidity below 60% RH, but surface moisture from condensation should be removed by drying at 70–80 °C for 1–2 hours using a desiccant dryer with a dew point of −30 °C or lower.
On single-screw extruders with L/D ratios of 24:1 to 30:1, the high-melt-index grade commonly lowers head pressure by 15–30% relative to a 20-MFI LLDPE at constant screw speed. This pressure reduction is observed on production lines but must be verified for each screw design because barrier screws and Maddock mixers generate different viscous heat. Documented production failure modes include die-lip plate-out when down-gauging below 0.5 mm at high line speed, and screw slippage when feed-throat temperature exceeds 60 °C because the granule bed loses frictional conveyance.
As a carrier resin for color or additive concentrates, the high melt index allows twin-screw compounding on corotating extruders with L/D 40:1 to 48:1 and screw speeds of 300–800 rpm. Calcium carbonate loadings of 60–75 wt% and carbon black loadings of 25–50 wt% are processable when distributive mixing elements are used after the first kneading block. Published data for this specific configuration is limited because concentrate viscosity depends on additive surface area, carrier melt viscosity, and screw profile. The low viscosity of PE100LLD-50M reduces motor torque at high filler loading, but it also reduces melt-phase dispersion intensity; therefore, a two-stage screw with a vacuum vent at −0.08 MPa gauge is recommended to remove moisture and low-molecular-weight volatiles.
Capillary rheometry under ASTM D5422-19 or ISO 11443:2021 is the appropriate method for viscosity-shear-rate mapping. For a 50-MFI LLDPE at 190 °C, apparent shear viscosity can be expected to fall from the order of 1,000 Pa·s at 100 s−1 to below 100 Pa·s at 1,000 s−1; exact curves depend on comonomer type, polydispersity, and additive package. Differential scanning calorimetry under ASTM D3418-21 typically shows a crystalline melting peak between 120 °C and 128 °C and a crystallization exotherm near 104–110 °C for linear low density polyethylene; these ranges are class-typical, not product-specific guarantees. Screw designs for LLDPE generally favor compression ratios of 2.5:1 to 3.5:1 and a feed depth that maintains a solid bed before compression; deep metering channels reduce shear heating for this low-viscosity grade.
Published data for CP Pryme PE100LLD-50M were not fully reproduced in the source material; the following numeric windows are class-typical values for 50-MFI linear low density polyethylene derived from ASTM-referenced trade literature and are not a purchase specification.
| Property | Test Method | Class-Typical Range for 50-MFI LLDPE |
|---|---|---|
| Melt mass-flow rate | ASTM D1238-20 / ISO 1133-1:2022 | 190 °C/2.16 kg; nominal 50 g/10 min |
| Density | ASTM D792-20 / ISO 1183-1:2019 | 0.915–0.940 g/cm³ |
| Tensile stress at yield | ASTM D638-22 / ISO 527-2:2012 | 8–14 MPa |
| Elongation at break | ASTM D638-22 | 200–800% |
| Flexural modulus | ASTM D790-17 / ISO 178:2019 | 200–600 MPa |
| Vicat softening temperature | ASTM D1525-17e1 | 85–110 °C |
| Environmental stress-crack resistance | ASTM D1693-21 | published data for this specific configuration is limited |
In cast film and extrusion coating, the low melt viscosity is used to reduce neck-in and promote high line speed at low coating weight. A typical cast film configuration uses a coat-hanger die with a die gap of 0.5–0.8 mm, chill-roll temperatures of 15–25 °C, and melt temperatures at the die lip between 210 °C and 240 °C. Under these conditions, a 50-MFI LLDPE permits draw-down to coating thicknesses below 10 µm; however, heat-seal initiation temperature and hot-tack strength must be re-qualified because these properties shift with comonomer type, density, and molecular weight. In blown film, the grade is not the first choice for high-bubble-stability applications; the low melt strength tends to produce bubble instability at blow-up ratios above 2.5:1 unless blended with LDPE or a lower-MFI LLDPE.
Direct substitution of a 20-MFI linear low density polyethylene with PE100LLD-50M requires recalculation of the injection velocity profile and cushion. The lower viscosity shortens fill time at equivalent machine settings but also raises the risk of flash in multi-cavity tools with parting-line wear. Processors report needing to reduce holding pressure by 10–25% and shorten holding time by 20–40% on polypropylene-style hot-runner manifolds when melt-flow index doubles from 20 to 50 g/10 min. Gate freeze-off occurs later because the lower-molecular-weight resin remains molten longer at the gate; if the holding phase is not shortened, sink marks and dimensional warpage increase. The part may also show reduced impact resistance under ASTM D256-23e1 and reduced tensile elongation under ASTM D638-22; these reductions must be measured on production parts, not on generic plaques.
Food-contact status must be confirmed with Chase Plastics for the specific lot because olefin polymers can be covered under FDA 21 CFR 177.1520(c) when the base resin meets the prescribed density and extraction limits. The product is subject to REACH under Regulation (EC) No 1907/2006 and must be evaluated for SVHC content if imports into the European Union are considered. Under RoHS 2011/65/EU, polyolefin resins are generally outside the scope of restricted substances when used in electrical and electronic equipment parts, but downstream converters must verify added flame retardants, pigments, or metal-based additives. Compliance with ASTM D3350-21 cell classification is not automatic for this general-purpose grade; pressure pipe or gas distribution service requires product-specific hydrostatic design basis data that Chase Plastics may not provide for this grade.
A frequent misapplication is the replacement of a 1.0-MFI octene LLDPE with a 50-MFI LLDPE in cold-impact packaging on the assumption that density is equivalent. The molecular weight difference produces lower entanglement density, which reduces dart impact under ASTM D1709-16a and instrumental puncture under ASTM D5748-19. For freezer applications operating below −20 °C, the brittle-ductile transition may shift upward by several degrees, increasing the probability of fracture during drop testing. Published data for this specific configuration is limited, but class-typical low-temperature Izod impact values for 50-MFI LLDPE are commonly lower than those of 20-MFI material by 20–50%. Applications that require long-term slow-crack-growth resistance, such as rotationally molded tanks or geomembranes, should not be designed around this grade without a full ASTM F1473 test program.
If the grade is considered for rotational molding, the low melt viscosity at peak internal air temperature may cause pinhole formation in complex mold geometries; published data for this specific configuration is limited. Rotational molding processors characteristically prefer linear low density polyethylene with melt indexes between 3 and 8 g/10 min under ASTM D1238-20. At 50 g/10 min, the reduced melt elasticity shortens sintering time but produces thinner wall coverage on deep ribs. Addition of 0.1–0.5% high-temperature antioxidant may be required to limit oxidative degradation at oven temperatures near 300 °C; the stabilizer package should be evaluated by differential thermal analysis under ASTM D3895-19.