| HS Code | 286772 |
| Reinforcement | 30% glass fiber |
| Density | 1.53 g/cm³ |
| Tensile Strength | 140 MPa |
| Elongation At Break | 2.5% |
| Flexural Strength | 200 MPa |
| Flexural Modulus | 8500 MPa |
| Notched Izod Impact Strength | 80 J/m |
| Heat Deflection Temperature At 1 82 Mpa | 210 °C |
| Melting Point | 225 °C |
| Mold Shrinkage | 0.2-0.5% |
| Water Absorption At 24 H | 0.04% |
| Volume Resistivity | 1E16 Ω·cm |
| Dielectric Constant At 1 Mhz | 3.5 |
| Flammability | UL 94 HB |
As an accredited Chang Chun LONGLITE® PBT+GF 4830 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Chang Chun LONGLITE® PBT+GF 4830 is supplied in 25 kg moisture-resistant bags, palletized for industrial delivery. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with palletized 25 kg bags of Chang Chun LONGLITE® PBT+GF 4830, stretch-wrapped and secured for export. |
| Shipping | Chang Chun LONGLITE® PBT+GF 4830 is shipped as non-hazardous, moisture-sensitive thermoplastic resin pellets in sealed bags or bulk containers. Transport and store in cool, dry conditions, away from direct sunlight, heat, and contamination. No UN hazardous-goods classification applies. |
| Storage | Store Chang Chun LONGLITE® PBT+GF 4830 in a cool, dry, well-ventilated area away from direct sunlight, heat, ignition sources, and moisture. Keep original containers tightly sealed, palletized, and off the floor. Prevent humidity absorption, dust generation, and static buildup; follow first-in, first-out stock rotation. |
| Shelf Life | Typically 24 months in original unopened packaging when stored cool, dry, and protected from moisture, heat, and direct sunlight. |
LONGLITE® PBT+GF 4830 is transferred directly from closed-loop desiccant drying into underhood electrical connector production cells as a 30 wt% short-glass-fibre-reinforced polybutylene terephthalate compound. Drying is maintained at 120 °C to 130 °C with a dew-point floor of -30 °C; hopper residence times of 3 h to 4 h are used to force residual moisture below 0.02 %. Production failures observed on 40 mm screw-diameter reciprocating units with L/D ratios of 20:1 to 24:1 occur when overnight material is left under ambient relative humidity above 60 %; hydrolysis-induced molecular weight reduction then generates gas-void porosity near gate pucks and lowers the notched Charpy impact result below 7 kJ/m². The glass-fibre addition ratio remains fixed at 30 %, while reprocessed sprues and runners are capped at 20 % of total shot mass for connector housings because repeated melt histories reduce fibre length below the critical transfer length and weaken the terminal lock arm, especially at knit lines with glass depletion.
Compliance for engine-bay connector applications is anchored to ISO 527-2:2012 tensile evaluation, ISO 178:2019 flexural testing, ISO 75-2:2013 heat deflection temperature at 1.8 MPa, and USCAR-2 mechanical and environmental performance classes where the PBT-GF30 grade is selected for 125 °C continuous use under Class T3; assignment to 150 °C Class T4 is not supported for continuous exposure. Glow-wire testing is performed to IEC 60695-2-11 at 750 °C on finished wall thicknesses, and vertical-burn classification follows UL 94 per the lot card. The production route is injection moulding through hot-runner valve gates with melt temperature 250 °C to 270 °C and mould temperature 60 °C to 100 °C; the upper mould-temperature band is applied for thin-wall terminal retention sections below 1.0 mm to delay frozen-layer growth. Flow-front velocity is controlled at 100 mm/s to 250 mm/s, and cavity packing pressure is held at 60 MPa to 80 MPa for 6 s to 12 s. Mould shrinkage is anisotropic, reading 0.2 % to 0.4 % in the flow direction and 0.8 % to 1.0 % transverse, so connector pin-hole concentricity is maintained by asymmetric tool cooling rather than by post-mould fixturing. Terminal finished product types include engine control unit connector shells, transmission speed sensor housings, fuse-box high-current terminal carriers, and in-line harness connectors for 12 V and 48 V electrical architectures.
Battery management system interconnects moulded from LONGLITE® PBT+GF 4830 are specified where the part must withstand 85 °C/85 % relative humidity damp-heat exposure and 125 °C peak dry-heat exposure while retaining dielectric strength. The primary compliance boundary is IEC 60664-1:2020 creepage and clearance coordination; comparative tracking index testing under IEC 60112:2020 determines the maximum allowable working voltage across terminal spacings on the connector body. Glow-wire end-product testing to IEC 60695-2-11 is performed at 850 °C for accessible surfaces, and the flame-retardant package of the compound maintains UL 94 V-0 down to the certified wall thickness when final parts are burned in the as-moulded condition. The 30 wt% glass-fibre loading produces a flow-direction coefficient of linear thermal expansion near 2.2 × 10⁻⁵ K⁻¹ to 2.8 × 10⁻⁵ K⁻¹, reducing terminal loosening under thermal cycling compared with unfilled PBT; however the glass-fibre surface also creates local electric field amplification at fibre-resin interfaces, so comparative tracking index values are inherently lower than the unfilled resin and lot-to-lot variation must be monitored. No downstream addition or reprocessing is permitted for high-voltage interlock connector bodies because any re-compounding can disturb the flame-retardant synergist distribution and shift comparative tracking index by more than 100 V.
Production tooling for battery management system carrier frames uses sequential valve gating on four to eight drops, with melt temperature limited to 255 °C to 265 °C and mould temperature 80 °C to 110 °C; the elevated mould temperature promotes crystallinity and reduces moisture regain in damp-heat testing. Screw back-pressure is set at 0.5 MPa to 1.0 MPa to disperse glass bundles without exceeding residence time; barrel residence time is kept below 5 min at full barrel capacity to avoid polyester thermal degradation. Packing pressure profiles use 60 % of injection pressure for 8 s then decay to 30 % for 4 s; this sequence controls sink in terminal standoffs and minimises post-mould warpage across 120 mm connector lengths. Terminal finished products include battery management system slave module frames, cell-monitoring unit mounting rails, charging inlet control pilot connector bodies, and high-voltage interlock terminal carriers. For applications requiring continuous exposure above 150 °C or dielectric withstand above 1000 V AC after 1000 h at 125 °C, the disclosed design guide replaces PBT-GF30 with PA66-GF30 or PPS, because polyester embrittlement and surface hydrolysis create leakage-current paths across contaminated glass-rich surfaces. Published data for this specific connector configuration is limited; lot qualification is performed on a part-specific basis.
Miniature circuit breaker bodies and bases require a combination of dimensional stability, low post-mould moisture uptake, and arc-quenching surface integrity. LONGLITE® PBT+GF 4830 is case- and base-moulded with the 30 wt% short-glass-fibre content retained at the compound level; regrind is excluded for surfaces adjacent to the arc splitter plates because recycled glass bundles create local dielectric discontinuities that can initiate tracking failure during short-circuit interruption tests. Compliance is evaluated to IEC 60898-1:2015 for household miniature circuit breakers, IEC 60947-2 for industrial switchgear enclosures, and IEC 60695-2-11 glow-wire testing at 960 °C on the external face. Material certification also references IEC 60695-2-12 and IEC 60695-2-13 glow-wire ignition and ignitability limits for unattended appliances carrying more than 0.2 A.
Tooling is multi-cavity with tangential edge gates located away from the arc chamber walls. Melt temperature is held between 250 °C and 260 °C; mould temperature is raised to 90 °C to 110 °C to stabilise crystallinity and maintain arc-track resistance and the 0.1 mm flatness over 60 mm terminal pad length. Injection speed is set to achieve a flow-front velocity at the arc chamber rib of 120 mm/s to 180 mm/s; higher speeds create jetting and glass-fibre orientation perpendicular to the flow that increases transverse shrinkage to 1.2 % and causes local warpage near the solenoid trip window. Post-mould, parts are annealed at 100 °C for 2 h to reduce residual stress and then conditioned at 23 °C/50 % RH for 48 h before dimensional audit. Tool wear from 30 % glass fibre is observed as gate erosion after 80,000 to 120,000 shots on hardened gate inserts; shot-to-shot variation in terminal pad flatness increases by 0.03 mm across this interval. Terminal product types include miniature circuit breaker bodies and bases, residual-current device housings, modular contactor arc chambers, and terminal strip bases used in distribution boards.
Cooling fan blades and shroud moulding with LONGLITE® PBT+GF 4830 imposes a separate set of constraints because the part is rotationally dynamic and must survive vibration, thermal cycling, and occasional hot coolant splash. The 30 wt% glass-fibre content raises flexural modulus to 8,000 MPa to 9,500 MPa under ISO 178:2019, but weld-line fatigue at the hub-to-blade junction remains the controlling acceptance criterion. Compliance is evaluated through ISO 527-2, ISO 179-1/1eA, and ISO 75-2; assembled fan balance is verified against OEM-specific residual unbalance limits rather than a single ISO standard. No more than 10 % clean runner regrind is used because blade-weight variation must remain within ±1.0 % and recycled material shifts the mass distribution enough to affect balance. Production tools use centre sprue gating into the hub to keep the weld line at the hub rather than the blade, with melt temperature 255 °C to 270 °C and mould temperature 80 °C to 100 °C. Holding pressure is set at 50 MPa to 70 MPa; cycle times run 45 s to 70 s depending on wall thickness between 2.0 mm and 3.5 mm. In production, imbalance failures are traced to glass migration at the rib-blade junction; moulders increase screw back-pressure to 1.0 MPa and reduce injection velocity by 15 % to reduce free glass at the surface. Terminal finished product types include engine cooling fan blades, fan shroud rings, cowl extensions, and HVAC blower wheel hubs. Continuous exposure to coolant splash above 130 °C is outside the material boundary; PA66-GF30 or polyphenylene sulphide is substituted in those thermal zones.
In power tool gear housings and motor brackets, PBT+GF 4830 is used for its high stiffness-to-weight ratio and dimensional predictability, but the main process conflict arises where rib roots intersect bearing bores. The 30 wt% glass-fibre reinforcement increases heat deflection temperature to the 200 °C to 210 °C band at 1.8 MPa under ISO 75-2:2013, allowing gearbox temperatures generated by lithium-ion motor packs to be tolerated without creep-induced bore ovalisation. Safety compliance follows EN IEC 62841-1:2018 for motor-operated hand-held tools, with material flammability accepted at UL 94 V-0 per final part thickness. Rib geometry is constrained by the compound’s shrink behaviour: nominal wall thickness is held at 2.5 mm to 3.0 mm, and rib thickness is kept below 40 % of the adjacent wall to avoid sink marks; the 30 wt% glass content reduces total mould shrinkage to 0.3 % flow and 1.0 % transverse, but differential packing pressure decay between the bearing bore and rib root creates sink if gate freeze-off is reached early.
Two-stage injection controls velocity at 80 mm/s to 120 mm/s for the first 60 % of fill, then reduces to 40 mm/s through bearing core pins to prevent glass-fibre breakage at the bore surface. Melt temperature is held between 250 °C and 265 °C, mould temperature at 70 °C to 90 °C, and packing is applied at 70 MPa for 5 s followed by 35 MPa for 10 s; the extended lower-pressure hold compensates for volume shrinkage in the rib-root region. Production lines with gas-counterpressure or external gas pin systems are not recommended because the grade’s flame-retardant package forms plate-out on venting surfaces under gas-assisted operation. Terminal finished product types include angle grinder gear housings, drill motor bearing brackets, circular saw blade guards, and cordless impact driver transmission covers. Drop-test failure above 2 m on concrete is common if ribs exceed 50 % of nominal wall thickness; impact-modified PBT or polycarbonate blend is substituted in such designs.
Circulation pump housings in domestic appliances are a substitution zone where PBT+GF 4830 replaces modified polyphenylene oxide and sometimes polyphenylene sulphide for non-boiling water loops up to 95 °C. The 30 wt% glass-fibre addition ratio is fixed in the compound and gives creep resistance under the radial load of the impeller at 3,000 rpm to 6,000 rpm, resisting deformation of the volute tongue in continuous circulation service. Compliance under IEC 60335-1:2020 household appliance safety governs electrical insulation of the pump body, and NSF/ANSI 61 applies when the pump has incidental contact with potable water; published data for repeated boiling-water pressure cycles in this specific grade is limited, so the material is restricted to systems with thermal cut-out below 100 °C and pH between 5.5 and 8.5 to avoid polyester hydrolysis. Regrind is capped at 15 % for non-wetted housings and excluded entirely for wetted pump bodies because glass-rich regrind surfaces reduce ultrasonic weld energy transmission at the volute-to-cover joint.
The pump housing is injected with melt temperature 245 °C to 265 °C and mould temperature 80 °C to 100 °C; the gate is positioned at the hub core to establish a glass-fibre orientation that follows the volute spiral and prevents a knit line at the volute tongue. Injection speed is set at 60 mm/s to 100 mm/s to avoid gas entrapment at the blade clearance rib, and packing pressure is held at 55 MPa for 7 s. Post-mould dimensions are audited after 24 h annealing at 85 °C because PBT continues secondary crystallisation for the first day after moulding; the impeller-to-housing clearance is designed around 0.2 % to 0.4 % post-shrink in the volute diameter. Terminal finished products include central heating circulator pump bodies, dishwasher wash pump impellers, washing machine drain pump volutes, and sensor connection flanges in domestic water-management systems. The substitution is not valid for steam condensate loops above 110 °C or alkaline cleaner exposure with pH above 10, where hydrolysis-resistant grades or stainless steel are used.
Competitive Chang Chun LONGLITE® PBT+GF 4830 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chang Chun LONGLITE® PBT+GF 4830 is supplied as a 30% glass-fibre-reinforced polybutylene terephthalate injection moulding grade. The 4830 designation identifies the 30 wt% glass-reinforced member of the LONGLITE® PBT product family in supplier documentation. The matrix is a semicrystalline polyester with rapid crystallisation, low equilibrium moisture uptake, and selective chemical resistance, while the short glass-fibre reinforcement raises tensile strength, flexural modulus, and heat deflection temperature relative to unfilled PBT. The compound is intended for reciprocating-screw injection moulding of dimensionally stable parts in electrical, automotive, and pump systems. Density measured under ISO 1183-1:2019 is typically 1.52–1.55 g/cm³.
Mechanical property determinations are reported at 23°C and 50% relative humidity after conditioning according to ISO 291. Tensile strength at break under ISO 527-2 is typically 125–135 MPa, with tensile elongation at break of 2.0–3.0%. Flexural modulus under ISO 178 is typically 8,500–9,500 MPa, and flexural strength is typically 180–200 MPa. The grade therefore occupies the upper stiffness range for non-flame-retardant PBT compounds with a nominal 30 wt% glass loading. Property retention after prolonged thermal exposure is grade-specific and should be confirmed from the supplier’s UL yellow card for the specific colour and wall thickness.
Shrinkage anisotropy is significant in this grade. Injection-moulded plaques tested under ISO 294-4 commonly show flow-direction shrinkage of 0.2–0.5% and transverse shrinkage of 0.7–1.0%. The anisotropy follows fibre orientation at the melt front and is influenced by mould temperature, hold pressure, and gate geometry. Tool designers using uniform shrinkage allowances for unfilled PBT will produce undersized or warped parts when switching to the 30% glass grade; cavity dimensions should be corrected through iterative mould trials or supplier shrinkage data at the actual wall thickness.
In load-bearing applications, the grade is selected for elevated modulus at temperatures approaching 200°C under short-term no-load conditions. The heat deflection temperature under 1.82 MPa load and ISO 75-2 is typically 195–205°C. Continuous service temperature is lower; unfilled PBT relative thermal index values under UL 746B are commonly below 120°C, and the glass-reinforced grade should be evaluated on a thickness-dependent basis rather than assumed. Weld-line strength retention is a limiting factor. When two flow fronts combine downstream of a core or in multi-gate filling, tensile strength retention measured on double-end-gated plaques under ISO 527-2 is commonly 50–65% of the un-welded value. For pressure-containing housings, gate locations should be arranged to move weld lines away from hoop-stress regions.
Specimen geometry affects the reported values. Tensile modulus is determined on ISO 1A or 1B specimens at a crosshead speed of 1 mm/min; flexural modulus is determined on 80 × 10 × 4 mm bars at 2 mm/min; notched Izod impact is measured on Type 1A bars with a notch radius of 0.25 mm after conditioning at 23°C and 50% relative humidity. Apparent modulus values may shift lower when wall thickness drops below 2 mm because of skin-core fibre orientation. Design calculations for thin-wall housings should therefore use thickness-corrected modulus values obtained from injection-moulded plaques rather than datasheet values from 4 mm tensile bars.
| Property | Test method | Typical value |
|---|---|---|
| Density | ISO 1183-1:2019 | 1.52–1.55 g/cm³ |
| Tensile strength at break | ISO 527-2 | 125–135 MPa |
| Tensile elongation at break | ISO 527-2 | 2.0–3.0% |
| Flexural modulus | ISO 178 | 8,500–9,500 MPa |
| Flexural strength | ISO 178 | 180–200 MPa |
| Notched Izod impact, 23°C | ISO 180/A | 7.0–9.0 kJ/m² |
| Heat deflection temperature, 1.82 MPa | ISO 75-2 | 195–205°C |
| Melt mass-flow rate, 250°C/2.16 kg | ISO 1133-1:2022 | 15–25 g/10 min |
| Mould shrinkage, flow direction | ISO 294-4 | 0.2–0.5% |
| Mould shrinkage, transverse direction | ISO 294-4 | 0.7–1.0% |
| Volume resistivity | IEC 60093 | 1 × 10^15 Ω·cm |
| Comparative tracking index | IEC 60112 | 250–300 V |
| Flame rating | UL 94 | HB at 1.5 mm and 3.0 mm |
Notched impact strength under ISO 180/A is typically 7.0–9.0 kJ/m² at 23°C. This value indicates that PBT+GF 4830 is not a high-toughness grade; sharp corners, snap-fit arms, and screw bosses require generous radii. Fibre orientation and notch sensitivity also reduce effective impact resistance in the flow direction relative to cross-flow specimens. Impact values at −30°C are commonly 10–20% lower than room-temperature values for this class of material. Published low-temperature impact data for this specific configuration is limited and should be generated on production-thickness samples if cold-impact certification is required.
Moisture control is the first processing constraint. PBT undergoes hydrolytic degradation when melt moisture exceeds 0.02%; surface splay, embrittlement, and a measurable drop in melt viscosity appear before dimensional instability. The material should be dried in a desiccant dryer with a dew point no higher than −40°C at 120°C for 4–6 h. Hopper residence time should not exceed 8 h unless the hopper is blanketed with dry air. Moisture verification by coulometric Karl Fischer titration under ISO 15512:2019 is recommended for production-run approval.
| Processing parameter | Setting |
|---|---|
| Drying temperature, desiccant dryer | 120°C |
| Drying time | 4–6 h |
| Final moisture limit | <0.02% |
| Melt temperature | 240–270°C |
| Mould temperature | 60–100°C |
| Barrel rear zone | 230–240°C |
| Barrel middle zone | 245–255°C |
| Barrel front zone | 250–260°C |
| Nozzle | 255–265°C |
| Injection pressure | 60–100 MPa |
| Hold pressure | 40–70 MPa |
| Back pressure | 3–7 MPa |
| Screw speed | 60–120 rpm |
Barrel temperature mapping follows a rising profile from rear to nozzle. The rear zone is held at 230–240°C to avoid premature melting before compression; the front zone and nozzle are held at 250–265°C to prevent nozzle freeze-off. Melt temperatures above 270°C or residence times exceeding 8–10 min accelerate thermal degradation, producing yellowing, acrid volatiles, and black specks. Screw speed above 120 rpm on general-purpose screws with 20:1–22:1 L/D increases fibre breakage and reduces mechanical property retention. Screw speed must be matched to shot size so that plastication time remains below cooling time in automatic cycles.
Mould temperature influences surface finish and crystallinity. At mould temperatures below 60°C, parts may exhibit visible flow lines and reduced property uniformity; at temperatures above 100°C, cycle time increases and ejection may be complicated by lower hot-tear resistance. Production-scale experience on toggle-clamp machines of 80–120 t shows that hold pressure below 40 MPa at rib intersections produces sink marks and dimensional drift. Cavity pressure decay monitoring is recommended; if cavity pressure at the gate falls to zero before the part freezes, hold pressure should be increased or gate dimensions enlarged. Masterbatch addition should be dry-blended before hopper loading.
Electrical terminal blocks, automotive relay housings, cooling-fan frames, and pump impellers represent the principal production applications where this 30% glass-reinforced grade is substituted for unfilled PBT or lower-glass PBT. This substitution is driven by dimensional stability and elevated stiffness rather than toughness. Compared with unfilled PBT, the 30% glass grade raises flexural modulus from roughly 2,500–3,000 MPa to 8,500–9,500 MPa and raises HDT/A from roughly 50–60°C to 195–205°C. The same substitution reduces unfilled PBT mould shrinkage from 1.5–2.0% to 0.2–0.5% in the flow direction, but transverse shrinkage remains higher and fibre orientation causes anisotropic warpage. Compared with PBT grades containing 15% or 20% glass, the 4830 grade provides higher modulus and heat deflection temperature but shorter spiral-flow length and lower weld-line strength retention.
Electrical applications utilise the volume resistivity and tracking resistance of the compound. Volume resistivity under IEC 60093 is typically 1 × 10^15 Ω·cm, and comparative tracking index under IEC 60112 is typically in the 250–300 V range. These values support medium-insulation coordination in dry environments; condensate-prone or heavily polluted applications require additional creepage distances or a flame-retardant, higher-CTI grade. The material is normally supplied with a UL 94 HB classification at thicknesses of 1.5 mm and 3.0 mm. Components requiring V-0 should specify a flame-retardant PBT because the 30% glass content lowers ignition resistance relative to unfilled PBT.
Chemical resistance is selective. Weight and dimension changes after immersion in aliphatic hydrocarbons and mineral oils at 23°C under ISO 175 are generally small, but chlorinated hydrocarbons, strong acids, and alkaline solutions attack the polyester matrix. Continuous hot-water service above 80°C is not recommended because hydrolysis reduces molecular weight and causes progressive embrittlement. Amine-based additives and alkaline processing aids should be avoided; ester-amide interchange and alkaline hydrolysis can occur in the melt and during component service.
For connector housings exposed to short-term peak temperatures during infrared reflow or engine-compartment soak, the specified HDT/A of 195–205°C does not by itself guarantee survival. The part design should be evaluated using supplier glass-transition and melt-temperature data, moulded-in stress levels from finite-element filling simulation, and thermal cycling profiles under ISO 16750-4 if automotive use is intended. In such applications, published multi-temperature creep data for this specific configuration is limited, and pilot mould trials on production tools with the final colour and thickness are required before release.