| HS Code | 328110 |
| Density G Cm3 | 1.55 |
| Glass Fiber Content Percent | 30 |
| Tensile Strength Mpa | 100 |
| Elongation At Break Percent | 2.5 |
| Flexural Modulus Mpa | 8500 |
| Notched Charpy Impact Kj M2 | 6 |
| Heat Deflection Temperature 1 82mpa C | 200 |
| Ul94 Flame Rating | V-0 |
| Water Absorption 24h Percent | 0.05 |
| Molding Shrinkage Percent | 0.2-0.6 |
| Melting Point C | 225 |
| Dielectric Strength Kv Mm | 20 |
| Volume Resistivity Ohm Cm | 1E16 |
| Arc Resistance S | 120 |
As an accredited Chang Chun LONGLITE® PBT+GF 4830 BKF factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packed in 25 kg moisture-resistant bags, typically 40 bags per 1,000 kg pallet, clearly labeled for safe storage and transport. |
| Container Loading (20′ FCL) | 20′ FCL containing palletized 25 kg bags of Chang Chun LONGLITE® PBT+GF 4830 BKF, shrink-wrapped and secured for ocean shipment. |
| Shipping | Typically shipped as non-hazardous solid polymer pellets in sealed moisture-barrier bags or boxes, palletized and stretch-wrapped. Store dry, cool, and ventilated; protect from sunlight, moisture, and contamination. Use original packaging and follow the supplier SDS and local shipping regulations. |
| Storage | Store in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep containers or bags tightly closed to prevent moisture absorption and contamination. Stack securely, avoid dust generation, and maintain good housekeeping. Do not store near strong oxidizers. Use appropriate PPE and follow the supplier’s SDS and local regulations. |
| Shelf Life | Typically 12 months from date of manufacture when stored dry, cool, and in unopened original packaging. |
In engine-compartment connector production, the compound is dried in a desiccant dryer with a −40 °C hopper-air dew point at 120 °C for 4 h until residual moisture falls below 0.02 wt% by Karl Fischer titration; wet PBT above 250 °C undergoes hydrolytic chain scission that lowers weld-line burst pressure and increases terminal-retention failure after thermal cycling. LONGLITE® PBT+GF 4830 BKF is run at 100% dry compound in connector applications, with up to 15 wt% clean sprue/runner regrind introduced only after the regrind has been re-dried to the same moisture limit and checked for melt-flow stability per ISO 1133-1:2022, because repeated regrind extrusion shortens glass-fibre number-average length beyond 0.4 mm and degrades pin-zone mechanical integrity. Process conditions on a 20:1 L/D general-purpose screw are melt temperature 255–265 °C, mould temperature 80–95 °C, peak cavity pressure 60–80 MPa measured by cavity-pressure sensors, back pressure 2–5 bar, screw cushion 3–5 mm, and injection speed controlled by screw-position switchover at 0.4 s after the pre-fill cushion; gates are positioned into thick bosses rather than directly onto pin arrays to prevent jetting and glass-fibre orientation defects at the terminal root, and barrel residence time is not permitted to exceed 8 min at 265 °C. Compliance verification for engine-compartment connectors follows USCAR-2 Revision 7 for terminal retention and contact resistance after thermal shock, ISO 16750-5 for chemical exposure to engine oil, coolant, road salt, and battery acid, RoHS Directive 2011/65/EU Annex II, and IEC 60112 for comparative tracking index; flammability classification is taken from the UL Yellow Card at final part thickness rather than from a nominal PBT-GF30 datasheet because unfilled and glass-filled PBT grades without a halogenated FR package are typically HB under UL 94, not V-0. Terminal product types include ECU connector housings, camshaft position sensor enclosures, ignition coil primary connectors, alternator rectifier supports, and coolant-temperature sensor housings. A process boundary applies at continuous oil exposure above 135 °C, where PBT without heat-stabilizing additives may show surface crazing and should not be substituted for PBT/ASA or polyamide without additional validation.
Sink formation opposite bosses and stiffening ribs is the dominant defect when hand-held power tool housings are filled with LONGLITE® PBT+GF 4830 BKF, and it is controlled not by raising mould temperature alone but by a two-stage injection profile with a short high-pressure packing phase followed by a 1–2 s screw decompression. The grade is processed at 100% neat dry compound; a 5 wt% impact-modifier masterbatch addition reduces flexural modulus below 8500 MPa under ISO 178 and is therefore rejected for gear-case geometries where pinion-bearing seat stiffness governs noise, while a 10 wt% clean regrind fraction is the practical ceiling before notched Charpy impact scatter across shot-to-shot samples widens beyond the production-control limit of 15% of lot mean. Cylinder temperature is held at 250–270 °C, mould temperature at 60–80 °C, holding pressure at 45–60 MPa for 5–7 s, and screw speed on the 20:1 L/D glass-filled screw is limited to 60–100 rpm to limit glass-fibre attrition during plastication; bimetallic barrel and nitrided screw surfaces are specified because glass-fibre reinforced PBT increases screw and check-ring wear in continuous production. Enclosure compliance is assessed under IEC 62841-1 for hand-held motor-operated tools, UL 746C for polymeric enclosures in portable tools, and IEC 60068-2-75 for mechanical impact resistance at 0.5 J; dimensional stability after 4 h at 140 °C is checked by ISO 75-2 Method A to control bearing-hole ovality. Terminal product types include angle grinder gear cases, drill housing clamshells, electric screwdriver chassis, high-temperature brush-holder plates, and router base housings. The compound’s carbon-black pigmentation precludes bright laser marking commonly specified for power tool nameplates, so pad printing or hot-foil marking is selected; additional carbon-black masterbatch must not be added because flow-length variability widens moulding-mass balance across multi-cavity tools.
Because three-phase current interruption imposes a 110 K thermal shock gradient across insert-moulded copper busbars in low-voltage switchgear terminal carriers, residual-stress control is prioritized over maximum melt flow. LONGLITE® PBT+GF 4830 BKF is processed at 100% neat dry compound; if a converter blends 10 wt% unreinforced PBT to improve thin-rib fill for 0.6 mm snap-fit latches, published data for that modified configuration is limited, and the comparative tracking index per IEC 60112 plus tensile strength per ISO 527-2 must be re-verified because reducing glass content changes both surface tracking resistance and mechanical load capacity. Melt temperature is maintained at 250–260 °C, mould temperature at 70–90 °C, and brass or copper inserts are preheated to 120–140 °C by induction to reduce differential shrinkage and prevent microcracking at the parting line; the packing pressure is ramped down over 6–8 s rather than snapped off to avoid frozen-in stress around the metal surfaces, and cavity-pressure switchover is set at 45 MPa instead of time-based switchover to compensate for batch-to-batch melt-viscosity shift. Insulation coordination follows IEC 60664-1 pollution degree 2, dielectric strength is tested per IEC 60243-1 at 1 kV/s in transformer oil, and glow-wire ignitability is evaluated per IEC 60695-2-13 at final wall thickness rather than on a 3 mm plaque because glass-filled PBT does not inherently achieve the same glow-wire performance at every section. Terminal product types include DIN-rail terminal block insulators, contactor arc-chute supports, miniature circuit breaker bases, busbar insulating strips, and motor starter terminal carriers. Amine-based mould-release agents are incompatible because ester exchange accelerates surface hydrolysis and can reduce dielectric strength after humid ageing.
The critical manufacturing defect in axial-flow cooling fan production is not dimensional warpage alone but blade-to-blade mass imbalance caused by fibre-orientation discontinuity at the central gate. LONGLITE® PBT+GF 4830 BKF is therefore injected through a hub valve gate with a 0.5 s post-fill pack; the mould is held at 85–100 °C to promote crystallization and minimize post-mould warpage, while screw speed is limited to 60–100 rpm to preserve glass-fibre length in the melt. The resin is used at 100% virgin dry compound; regrind is kept at or below 10 wt% and homogeneously blended through a gravimetric feeder because cumulative fibre-length reduction shifts blade mass distribution and pushes residual unbalance outside balance grade G6.3 per ISO 21940-11, with many automotive cooling-module producers specifying G2.5 for tip speeds above 25 m/s. Compliance and durability verification includes ISO 21940-11 for residual unbalance, ISO 178 for flexural-modulus retention after 1000 h at 140 °C, ISO 899-2 for tensile creep at the hub, and ISO 75-2 Method A for heat-deflection temperature; automotive fan suppliers additionally impose thermal-cycle profiles per ISO 16750-4 at −40 °C to 120 °C to detect hub cracking after repeated cold start. Terminal product types include radiator cooling fan blades, HVAC blower wheels, condenser fan spiders, industrial blower impellers, and uninterruptible power supply cooling rotors. The material is not recommended for immersion in hot water or water-glycol mixtures above 70 °C without hydrolysis-resistant modification, because standard PBT grades lose flexural modulus faster in humid thermal cycling.
In ignition coil bobbin moulding, the 0.8 mm wall around the secondary winding pins becomes the characteristic filling limitation, so the injection machine is configured for flash-free filling at relatively low material temperature rather than excessive shear. LONGLITE® PBT+GF 4830 BKF is processed at 100% dry compound; adding more than 20 wt% post-industrial regrind is discouraged because winding tension of 0.5–1.0 N compresses the bobbin and any fibre-length heterogeneity increases diametrical creep under winding stress, which can loosen the secondary coil over thermal cycles. Melt temperature is set at 255–265 °C, mould temperature at 90–100 °C, holding pressure at 55–65 MPa for 8–10 s to minimize sink at terminal slots, and multi-cavity hot-runner manifolds are balanced to ≤2% filling imbalance across eight cavities to control wire-groove width. Insulation-system compatibility is assessed under UL 1446 for electrical insulation systems, transformer construction under IEC 61558-1, and thermal-class mapping under IEC 60085; dimensional stability after 24 h at 150 °C is checked by ISO 75-2 Method A to prevent terminal-slot closure. Terminal product types include ignition coil primary bobbins, power-transformer coil formers, relay coil bodies, solenoid valve coil jackets, and E-core fuse holders. Continuous exposure to transformer oil above 110 °C must be validated because certain ester-based dielectric fluids can plasticize PBT, and published data for this specific grade under long-term ester immersion is limited.
When aluminium is replaced by LONGLITE® PBT+GF 4830 BKF in fractional-horsepower industrial pump housings, the substitution is restricted to neutral or mildly acidic aqueous media between pH 5 and pH 9 at continuous temperatures not exceeding 70 °C. The compound is used at 100% neat dry compound; if pump moulders add 5 wt% of a hydrolysis-stabilizer masterbatch to extend hot-water resistance, published data for the modified matrix is limited, and the material must be re-qualified for tensile-property retention after immersion testing per ISO 175 in 10 wt% ethylene glycol at 60 °C. Tooling uses 4–6 mm nominal wall thickness with a ribbed backside rather than 10 mm monolithic sections to avoid internal voids and low crystallinity; melt temperature is controlled at 250–260 °C, mould temperature at 80–100 °C, and cooling time is extended to 20–30 s based on shot mass and wall section to allow sufficient crystallization before ejection. Material creep under sustained hydrostatic pressure is screened by ISO 899-2, chemical resistance by ISO 175 immersion, and overall equipment safety falls under Machinery Directive 2006/42/EC for complete pump assemblies rather than a material-specific standard. Terminal product types include chemical transfer pump volutes for weak acid circulation, impeller housings for neutral aqueous media, diaphragm pump liquid ends, filter housings for cooling water circuits, and magnetically coupled pump bodies. The grade is not suitable for strong alkaline solutions above pH 9, aromatic or chlorinated solvents, or fuel alcohols, and should not be used for potable-water contact unless the specific grade is separately approved.
Competitive Chang Chun LONGLITE® PBT+GF 4830 BKF prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chang Chun LONGLITE® PBT+GF 4830 BKF is a black-pigmented, flame-retarded polybutylene terephthalate injection moulding compound in which the glass fibre content is nominally 30% by mass. The grade belongs to the PBT+GF 4830 series, and the BKF suffix indicates the black colour and flame-retarded configuration; the unreinforced and non-flame-retarded PBT grades are not interchangeable with this material in components requiring suppression of ignition or tracking under electrical load. Published supplier data for PBT+GF 4830 BKF are typically generated according to ISO 1183-1, ISO 527-1/-2, ISO 178, ISO 179-1/1eA, ISO 75-1/-2, IEC 60112, and UL 94. The compound is used in electrical connector carriers, relay bases, motor brush-card housings, circuit-breaker components, and power-contact supports. Because the black flame-retarded configuration changes melt viscosity, mould deposit behaviour, and electrical tracking resistance, processing conditions and design calculations should not be transferred from natural or non-flame-retarded PBT/GF30 grades without verification.
Compared with unfilled PBT, the 30% glass fibre reinforcement reduces post-mould shrinkage and raises the heat deflection temperature into a range where dimensional stability can be maintained under short-term thermal excursions. Compared with PBT/GF30 without flame retardant, the flame-retardant package increases density, can reduce comparative tracking index, and can reduce melt flow. These differences are summarised in Table 1. The values are not a certificate of analysis; they represent product-class ranges used in material screening before supplier lot-specific data are available.
| Property category | Test method | PBT+GF 4830 BKF expected class range | Unfilled flame-retarded PBT class range |
|---|---|---|---|
| Glass fibre content | ISO 3451-1 | 30% nominal | 0% |
| Density | ISO 1183-1 | 1.65–1.72 g/cm³ | 1.45–1.50 g/cm³ |
| Tensile stress at break | ISO 527-1/-2 | 120–140 MPa | 50–65 MPa |
| Flexural modulus | ISO 178 | 9000–11000 MPa | 2400–2800 MPa |
| Charpy notched impact strength | ISO 179-1/1eA | 6–10 kJ/m² | 3–6 kJ/m² |
| Heat deflection temperature at 1.8 MPa | ISO 75-1/-2 | 195–210 °C | 60–80 °C |
| Flammability at 0.8 mm | UL 94 | V-0 | V-0 or HB depending on grade |
The ranges in Table 1 are representative of published industrial data for flame-retarded PBT/GF30 and unfilled flame-retarded PBT product classes. They are not a certificate of analysis and do not replace lot-specific test reports for PBT+GF 4830 BKF. The elongation at break of the glass-reinforced grade is typically below 3%, while unfilled flame-retarded PBT may exceed 10%; this difference requires removal of snap-fit features or redesign of interference fits if a conversion from unfilled PBT is made.
Polybutylene terephthalate hydrolyses through random chain scission at the ester linkages. If moisture is present at melt processing temperatures above 240 °C, molecular weight reduction can occur and is observed as a drop in melt viscosity, lower tensile strength, and reduced weld-line integrity. The material should be dried in a dehumidifying desiccant dryer with a dew point of -40 °C or lower. A drying window of 120 °C to 130 °C for 3 h to 4 h is standard for this product class. The target moisture content is below 0.02% by mass, measured according to ISO 15512. If ambient relative humidity exceeds 60%, opened bags should be consumed within 2 h or returned to the dryer. Overdrying at 130 °C for more than 6 h can degrade the flame-retardant system and cause screw deposit formation, black specks, and colour drift.
Barrel-temperature profiles in injection moulding are constrained by two limits: the need to obtain complete glass-fibre wet-out and the need to avoid flame-retardant decomposition. Typical start values for a three-section screw are hopper/zone 1 230–240 °C, zone 2 250–260 °C, zone 3 250–260 °C, and nozzle 250–270 °C. Melt temperature should be held below 270 °C; hot-runner systems with long residence times may require lower manifold temperatures to prevent black specks. In production-scale trials on a hydraulic machine with clamp force above 1200 kN, a screw with an L/D ratio of 22:1 and compression ratio of 2.5:1 provided stable plastication; injection speed was set in the range 60–120 mm/s, back pressure at 0.3–0.7 MPa, and screw speed at 60–120 min⁻¹. Mould surface temperatures of 60–90 °C are used to balance surface finish and crystallinity.
UL 94 V-0 is a small-scale material flammability classification, not a final component certification. For appliance and power-distribution components, the glow-wire test according to IEC 60695-2-12 at 750 °C or 850 °C is frequently specified on the final moulded part. Glass-fibre reinforced flame-retarded PBT can show thickness- and colour-dependent glow-wire behaviour because glass fibres produce local wicking and heat-transfer paths, and black pigmentation can influence surface ignition. Published data for PBT+GF 4830 BKF under IEC 60695-2-12 is limited. Component-level testing at the minimum wall thickness and worst-case colour is required; material datasheet values alone are insufficient for glow-wire compliance.
Electrical insulation performance in PBT+GF 4830 BKF is governed by surface contamination and glass-fibre exposure. The comparative tracking index is determined under IEC 60112; flame-retarded PBT/GF30 grades commonly fall in the 200–250 V range, while many non-flame-retarded PBT/GF30 grades can reach 400–600 V. Volume resistivity measured according to IEC 62631-3-1 is typically in the range 10¹⁴–10¹⁶ Ω·cm at 500 V for dry mouldings. Dielectric strength under IEC 60243-1 is commonly 15–20 kV/mm for 2.0 mm specimens. These values degrade with moisture uptake and surface contamination; for high-humidity service, post-mould cleaning and conditioning are relevant. Mineral-filled PBT grades with lower glass content may show better tracking resistance but lower flexural modulus and lower heat deflection temperature.
In thin-wall connector housings below 1.0 mm nominal wall thickness, glass-fibre orientation follows the filling pattern and creates anisotropic shrinkage. Weld lines in PBT/GF30 can retain only 50–70% of the weld-free tensile strength; tensile specimens measured to ISO 527-1/-2 are therefore not representative of failure at the weld line. Gates should be positioned so that weld lines are moved away from snap-fit features and electrical contact retention areas. Holding pressure is typically set at 60–80% of peak injection pressure to compensate for PBT crystallisation shrinkage; holding time should match gate freeze, not simply cushion decay. Overly long holding times in flame-retarded PBT/GF30 can increase residual stress around inserts and create microcracks in the glass-resin interface.
Regulatory compliance for electrical and electronic applications is evaluated against RoHS Directive 2011/65/EU, Annex II restrictions, and REACH Regulation (EC) No 1907/2006. Since the BKF suffix denotes a black flame-retarded compound, the flame-retardant chemistry determines whether the grade falls within halogen-free procurement requirements. Published data for this specific configuration is limited; the supplier declaration should be checked for IEC 61249-2-21 halogen content limits if halogen-free assembly is specified. Table 2 provides the compliance checklist format.
| Requirement | Reference | Typical evaluation point |
|---|---|---|
| Flammability classification | UL 94 | V-0 at 0.8 mm supplier datasheet |
| Heat deflection temperature | ISO 75-1/-2 | 195–210 °C at 1.8 MPa |
| Tensile and flexural properties | ISO 527-1/-2, ISO 178 | Lot-specific report values required for design |
| Comparative tracking index | IEC 60112 | 200–250 V class typical for flame-retarded PBT/GF30 |
| Glow-wire flammability index | IEC 60695-2-12 | Component-specific; not extrapolated from UL 94 |
| RoHS restrictions | 2011/65/EU Annex II | Supplier conformity declaration required |
| REACH SVHC notification | EC No 1907/2006 Article 33 | Supplier declaration required |
Before dimensional inspection, moulded parts should be conditioned for 24 h in a standard atmosphere of 23 ± 2 °C and 50 ± 5 % relative humidity in accordance with ISO 291. If components are to be exposed to humid service, dimensional changes should be evaluated after conditioning at 40 °C and 93 % relative humidity for 96 h because glass-fibre reinforced PBT absorbs moisture preferentially along the fibre-matrix interface. Dimensional inspection under these conditions is the application-specific validation point for connectors, relay bases, motor brush-card housings, and power-contact carriers.