| HS Code | 363951 |
| Polymer Type | PBT |
| Reinforcement | Glass fiber |
| Glass Fiber Content | 15% |
| Color | Black |
| Density | 1.41 g/cm³ |
| Tensile Strength | 95 MPa |
| Elongation At Break | 3% |
| Flexural Modulus | 5500 MPa |
| Flexural Strength | 150 MPa |
| Notched Izod Impact Strength | 6 kJ/m² |
| Heat Deflection Temperature At 1 82 Mpa | 200 °C |
| Melting Temperature | 225 °C |
| Flammability Rating | UL94 HB |
| Water Absorption | 0.07% |
| Mold Shrinkage | 0.4% |
| Dielectric Strength | 20 kV/mm |
| Volume Resistivity | 1E15 Ω·cm |
As an accredited Chang Chun LONGLITE® PBT+GF 4815 BK factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Chang Chun LONGLITE® PBT+GF 4815 BK is supplied in 25 kg moisture-resistant paper bags, palletized for safe industrial storage and transport. |
| Container Loading (20′ FCL) | 20’ FCL container loaded with Chang Chun LONGLITE® PBT+GF 4815 BK in palletized bags, securely stowed and sealed for export. |
| Shipping | Chang Chun LONGLITE® PBT+GF 4815 BK is a glass-fiber-reinforced black PBT resin supplied as pellets. Ship in sealed, moisture-barrier bags or drums under dry, cool conditions; protect from heat, sunlight, and contamination. Classified as non-hazardous for transport unless SDS states otherwise; follow local regulations and label per SDS. |
| Storage | Store Chang Chun LONGLITE® PBT+GF 4815 BK in a cool, dry, well-ventilated area, away from direct sunlight, heat, flames, and moisture. Keep original containers tightly closed and labeled; prevent dust generation and static buildup. Avoid incompatible chemicals, maintain good housekeeping, use first-in/first-out stock rotation, and follow the manufacturer’s SDS. |
| Shelf Life | Shelf life is 24 months when stored cool, dry, ventilated, in original sealed packaging, protected from direct sunlight. |
Low-voltage connector housings and sensor bodies in dry under-hood and cabin-harness zones are specified in Chang Chun LONGLITE® PBT+GF 4815 BK when the moulded part must retain terminal insertion force after 1,000 h thermal ageing at 125 °C in air, maintain dielectric strength above 20 kV/mm at 1.0 mm wall thickness according to IEC 60243-1, and limit moisture-induced pitch change to less than 0.05 % after 24 h immersion at 23 °C according to ISO 62. The carbon-black pigmentation of the BK grade is dispersed during compounding; because carbon black can reduce comparative tracking index measured according to IEC 60112, connector designs relying on CTI class IIIa or higher require end-product CTI confirmation on black lots. Pre-drying is performed in a desiccant dryer with inlet dew point not above −30 °C, set to 120 °C for 4 h to 6 h; granule moisture is verified below 0.02 % by Karl Fischer titration before the material enters the feed throat. Moulding is carried out on a 100-t clamp injection machine with a 30 mm three-zone screw at L/D 22:1; barrel temperatures are profiled from 250 °C at the rear zone to 270 °C at the nozzle, with melt temperature measured at 260 °C to 265 °C by immersion pyrometer. Tool temperature is held at 80 °C to 90 °C using turbulent-flow water lines. Injection velocity at the screw tip is set between 80 mm/s and 120 mm/s, switch-over to holding pressure occurs at 95 % volumetric fill, and holding pressure is maintained at 60 MPa to 80 MPa for 3 s to 5 s per millimetre of wall section. Back pressure is limited to 2 MPa to 4 MPa to avoid excessive glass-fibre attrition. Gate diameter below 0.8 mm is avoided unless a hot-runner valve gate is used, because premature gate freeze-off prevents adequate packing at terminal retention windows and causes sink marks. Production regrind is limited to 15 wt% of total shot weight; higher regrind ratios degrade Charpy notched impact and increase crack sensitivity on snap-fit retention beams. Qualification follows SAE/USCAR-2 for terminal retention and vibration, ISO 16750-4 for thermal cycling from −40 °C to 125 °C, and UL 94 HB for ignition resistance where the application does not require a flame-retardant material. This grade is not UL 94 V-0; a connector position requiring V-0 above 1.5 mm must use a designated flame-retardant PBT instead. Acceptance parts include seated sensor connectors, terminal position assurance caps, and harness-to-module interface housings.
Power tool motor brackets and brush holder plates produced from a 15 wt% glass-fibre PBT combine rigid screw bosses with wiring channels that thin to 1.0–1.2 mm, producing flow-length to wall-thickness ratios above 120:1. At these ratios, melt viscosity measured by ISO 11443 at 260 °C and 1,000 s⁻¹ should remain below 90 Pa·s for the black compound to fill a four-cavity cold-runner tool without jetting; if viscosity exceeds this range, shot weight variation across cavities increases beyond 0.15 %, and brush-slot width shifts by ±0.08 mm. Copper brush plates are preheated to 120 °C before insertion; the inserts must be degreased and free of silicone-based lubricants because surface contamination lowers overmoulded adhesion and promotes sink marks around the terminals. Tool temperature is held at 90 °C to improve glass-fibre wetting and reduce birefringence around insert edges. A clamping force margin of at least 15 % above projected cavity pressure is maintained to prevent flash at the parting line; projected cavity pressure is calculated from a maximum cavity pressure of 70 MPa over the projected area of the runner and parts. Hold pressure is set 20 MPa below peak cavity pressure to avoid overpacking the thin channel, which would cause warpage of the brush-slot datum. The motor bracket is tested under IEC 60745-1:2006+A11:2010 for mechanical strength and resistance to heat and fire; terminal-carrying parts that operate unattended may require a 750 °C glow-wire test according to IEC 60695-2-11. The non-flame-retardant 4815 BK may pass this glow-wire test only at end-product thickness; no V-0 classification should be assumed. Typical finished parts are brush holder plates and motor brackets for 600 W angle grinders and corded electric screwdrivers.
Solenoid bobbin flanges in pneumatic and hydraulic directional control valves are moulded with wall sections of 0.7–1.0 mm around a slender core pin that deflects under injection pressure above 120 MPa. Filling is split between two edge gates on the outer flange; the flow fronts meet at the core-pin side and create a weld line that must withstand coil-winding tension of 18–25 N applied on 0.6 mm enamelled copper wire. Core-pin steel is specified as 1.2343 ESR with a draft angle not below 0.5° and an ejector sleeve to avoid local core flex. Piezoelectric cavity-pressure transducers at the end of fill are used to trigger switch-over at 95 % of volumetric fill; peak cavity pressure in the thin bobbin flange is held below 80 MPa by reducing injection velocity in the last 15 % of stroke. Melt temperature is held at 270 °C to reduce anisotropic glass-fibre orientation, but residence time is limited to 5 min at 270 °C because thermo-oxidative degradation produces black specks, acetaldehyde odour, and a loss of weld-line elongation. The finished bobbin is tested for dielectric withstand at 1,500 V AC for 60 s after 48 h storage at 40 °C and 93 % relative humidity, following the creepage and clearance requirements of IEC 60947-5-1 for control circuit devices. If spacing calculation assumes pollution degree 2 and CTI class IIIa, the black grade must be verified under IEC 60112. The terminal component is a solenoid coil bobbin for a 3/2-way pneumatic pilot valve and a hydraulic valve coil assembly.
Screw-clamp and spring-clamp terminal blocks mounted on DIN rail in industrial control cabinets are produced from black 15 wt% glass-fibre PBT when the moulded body must hold brass conductor rails under wire tightening torque from 0.4 N·m to 1.2 N·m. The glass-fibre content is fixed at 15 wt%; local fibre depletion in screw-boss roots caused by sharp transitions below 0.4 mm radius aggravates comparative tracking index scatter by more than 30 V between cavities. Male brass inserts are preheated to 130 °C and moulded with a tool temperature of 100 °C to reduce fibre-poor surface layers around the metal. Melt temperature is kept at 265 °C, holding pressure at 65 MPa to 80 MPa. The terminal block body is evaluated under IEC 60947-7-1 for creepage distances and electrical clearances; comparative tracking index is tested according to IEC 60112. Where the end-product standard requires glow-wire ignition resistance, the moulded part is subjected to IEC 60695-2-11 at 750 °C for 30 s; acceptance is determined on the complete wall thickness, not on raw material plaques. Because the 4815 BK grade is not flame-retardant, connection blocks that must pass an 850 °C glow-wire test or a UL 94 V-0 rating require an alternative grade or a design with an intrinsic metallic barrier. Finished components include feed-through terminal bodies and fuse terminal bodies for 6.2 mm and 8.2 mm widths.
| Application segment | Pre-drying parameter | Granule moisture limit | Melt temperature | Tool temperature | Acceptance standard |
| Low-voltage automotive connector housing | 120 °C for 4–6 h | ≤0.02 % | 260–265 °C | 80–90 °C | SAE/USCAR-2; ISO 16750-4; UL 94 HB |
| Power tool brush holder plate | 120 °C for 4 h | ≤0.02 % | 260 °C | 90 °C | IEC 60745-1; IEC 60695-2-11 |
| Solenoid coil bobbin | 120 °C for 4–6 h | ≤0.02 % | 270 °C max | 90–100 °C | IEC 60947-5-1; IEC 60112 |
| DIN rail terminal block body | 120 °C for 4 h | ≤0.02 % | 265 °C | 100 °C | IEC 60947-7-1; IEC 60112; IEC 60695-2-11 |
| Dry environment relay socket | 120 °C for 4 h | ≤0.02 % | 260 °C | 85 °C | IEC 61810-1; UL 94 HB |
| Axial fan impeller | 120 °C for 4 h | ≤0.02 % | 265 °C | 100 °C | ISO 1940-1 |
In plug-in relay sockets and industrial control relay bases operating at 60–80 °C and low relative humidity, the low moisture uptake of PBT reduces pitch deviation compared with PA66. Under ISO 62, a 15 wt% glass-fibre PBT typically remains below 0.4 % moisture uptake after 24 h water immersion at 23 °C, whereas PA66 can exceed 6 % at saturation; this differential is relevant when terminal pitch is 5.0 mm and pin misalignment above 0.1 mm creates insertion force peaks. The 4815 BK grade is moulded in a two-cavity hot-runner tool with a central valve gate of 1.2 mm diameter; melt temperature is 260 °C and tool temperature is 85 °C. Hold pressure is applied at 70 MPa for 4 s per millimetre to pack the thick relay pin bosses without sink. After ejection, parts are placed on a flat cooling jig for 20 min to prevent post-moulding twist in the 55 mm length. Relay sockets are tested under IEC 61810-1 for clearances, creepage distances, and mechanical endurance; the insulating material is assigned UL 94 HB unless the equipment standard specifically requires V-0. The substitution of PA66 by this glass-fibre PBT is restricted to dry and intermittently humid environments because PBT undergoes hydrolytic degradation when exposed to water above 85 °C; steam-sterilised or hot-water-immersed relay bases require a hydrolysis-stabilised PBT or PPS. Terminal parts include octal relay sockets, DIN rail interface modules, and relay retaining clips.
Small axial fan impellers for telecom enclosures and server power supplies are moulded from black 15 wt% glass-fibre PBT when the end-user drawing specifies balance grade G 6.3 according to ISO 1940-1 and a blade-tip diameter of 80–120 mm. The material is processed with a central sprue gate at the hub, which creates radial glass-fibre orientation along each blade and can introduce residual stress that shifts blade-tip radial run-out after first heat-up. Granule pre-drying is performed at 120 °C for 4 h to a moisture content below 0.02 %; melt temperature is held at 265 °C and mould temperature at 100 °C to promote slow crystallisation and reduce differential shrinkage between hub and blade tip. Injection velocity is profiled from 45 mm/s in the hub to 90 mm/s in the blade ends, with holding pressure of 60 MPa and post-gate freeze time of 8 s. Ejected impellers are annealed in a circulating-air oven at 100 °C for 2 h and then cooled on a flat granite surface to room temperature before bore reaming. The bore is machined to a tolerance of H7 after annealing because moulded bore dimensions can change by 0.05–0.10 mm during relaxation of glass-fibre stresses. Balance and vibration testing uses ISO 1940-1 G 6.3; an unbalanced glass-fibre distribution caused by gate-induced orientation can raise vibration velocity above the acceptance limit of the fan assembly. Glass-fibre content above 15 wt% is avoided in these impellers because the additional fibre mass increases notch sensitivity at the blade root and reduces elongation at break. The finished product is an axial fan impeller for a 92 mm or 120 mm DC fan used in closed-loop power supply cooling.
Competitive Chang Chun LONGLITE® PBT+GF 4815 BK prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chang Chun LONGLITE® PBT+GF 4815 BK is a black, glass-fiber-reinforced polybutylene terephthalate injection-molding compound. The grade suffix 4815 BK is read within the LONGLITE PBT nomenclature as a nominal 15 wt% short-glass-fiber loading with black pigmentation, although the exact fiber mass fraction, glass sizing chemistry, and lot-specific melt viscosity must be verified from the current manufacturer technical datasheet. Published data for this specific configuration is limited outside the manufacturer’s controlled release; where numerical values are quoted below, they are class-reference ranges for injection-moldable PBT with the same nominal reinforcement level under the listed ISO methods, not guaranteed specification limits. The compound is intended for components that require higher stiffness and heat deflection temperature than unfilled PBT without the higher density and pronounced flow-direction anisotropy of a 30 wt% glass-fiber grade.
Molded test specimens should be produced according to ISO 294-1 and ISO 294-4 to obtain comparable shrinkage and mechanical data. Conditioning before testing is carried out under ISO 291 at 23°C and 50% relative humidity. Density measured by ISO 1183-1 immersion typically falls between 1.40 g/cm³ and 1.44 g/cm³ for a 15 wt% glass-fiber PBT class; water absorption under ISO 62 can approach 0.5% after equilibrium, which influences dimensions in humid service environments. Melt flow rate is determined by ISO 1133-1 at 250°C under 2.16 kg; the release value for the 4815 BK grade is not a universal constant because black pigment carriers can shift flow length and melt viscosity by several percent relative to an unpigmented control.
Tensile stress at break measured under ISO 527-2 at a crosshead speed of 5 mm/min for the 15 wt% glass-fiber PBT class is typically 90 MPa to 105 MPa, with tensile strain at break between 2.5% and 4.0%. Flexural modulus under ISO 178 is usually 5,000 MPa to 6,000 MPa, while flexural strength is approximately 140 MPa to 160 MPa. Heat deflection temperature obtained under ISO 75-2/A with 1.8 MPa applied stress lies between 200°C and 210°C; this is substantially above the 50°C to 60°C range for neat PBT. Notched Charpy impact strength under ISO 179-1/1eA at 23°C remains in the 4 kJ/m² to 6 kJ/m² range, which indicates that the material is still notch-sensitive and should not be selected where high-speed fracture energy is the primary requirement. Melting point determined by ISO 11357-3 is expected near 223°C, consistent with typical PBT homopolymer; the glass fiber does not alter the melting point but increases both melt stiffness and frozen-in orientation.
Shear-thinning behavior in a capillary rheometer indicates that apparent viscosity at 250°C and 1,000 s⁻¹ may be 30% to 40% lower than at 100 s⁻¹ due to glass-fiber orientation and matrix chain alignment. Screw torque during compounding follows the same trend; on a 25 mm parallel twin-screw extruder with a 40:1 L/D ratio, the specific mechanical energy input must be controlled below the level that promotes fiber attrition because excessive shear work reduces final tensile modulus. The glass-fiber aspect ratio retained in molded parts is a stronger predictor of flexural modulus than nominal fiber content, and the datasheet value alone is insufficient for critical load-bearing designs.
Batch-to-batch variation in black glass-filled PBT is typically lower in density and filler content than in colorant dispersion and melt flow rate. On a production injection machine, a melt flow rate drift of ±2 cm³/10 min under ISO 1133-1 can shift the pressure drop across a hot-runner valve gate by several percent and alter the packing window. For this reason, processors should not set the machine based on a single measured melt flow rate; the certificate of analysis trend chart and capillary flow data should be referenced when setting the initial barrel profile.
The material is highly sensitive to hydrolytic degradation when pellet moisture exceeds 0.02%. When storage relative humidity is above 60%, pre-drying in a desiccant dryer at 120°C for 4 h with a dew point not higher than -40°C is required before melt processing. A conventional hydraulic injection-molding machine with a 20:1 L/D general-purpose screw is adequate for moderate shot sizes, but check-ring non-return valves with glass-filled PBT require hardened surfaces because the short glass fibers accelerate wear. Barrel temperatures between 240°C and 260°C, a melt temperature of 250°C to 270°C, and a mold surface temperature of 60°C to 90°C balance flow length, crystallinity, and surface finish. Below 60°C mold surface temperature, weld-line strength deteriorates in thin-wall sections because the melt front solidifies before sufficient interdiffusion occurs; above 90°C, cycle time and post-crystallization shrinkage increase without proportional mechanical benefit. Hot-runner manifold and nozzle temperatures should remain within 250°C to 270°C, and total melt residence time should not exceed 5 minutes. Extended residence at 270°C causes black discoloration from thermal chain scission and molecular weight loss, which may not be visible but reduces tensile elongation at break.
Runner and gate sizing for the 15 wt% glass-fiber grade follows semi-crystalline PBT practice: circular cold runners should be at least 1.5 times the maximum wall thickness at the gate, and gate thickness should be 0.6 to 0.8 times the part wall. Smaller gates may increase shear heating and create surface silver streaks from volatile colorant carrier products. Valve-gated hot-runner systems require accurate temperature profiling; a nozzle tip temperature 10°C above the hot-runner manifold can cause localized melt degradation, while a tip temperature 10°C below the manifold may freeze glass-filled PBT at the gate during pack.
Post-molding dimensional change occurs because PBT continues to crystallize after demolding. At a mold temperature of 60°C, parts may show an additional 0.05% to 0.15% shrinkage within 24 h to 48 h after ejection; at 90°C mold temperature, crystallization is more complete in-tool and subsequent dimensional drift is lower. Dimensional audits for connector pitch and terminal retention holes should therefore be performed after aging, not immediately after molding.
Weld-line strength in glass-fiber PBT depends on gate count and location. In a dual-gated tensile bar molded according to ISO 527-2, the weld-line region can retain only 50% to 70% of the unwelded tensile strength because glass fibers align parallel to the melt front and do not bridge across the meeting plane. Mold surface temperature is the strongest single process variable, followed by injection velocity; increasing mold temperature from 60°C to 90°C may improve weld-line strength retention by 10% to 20% under otherwise constant conditions. For components with multiple sub-gates, the number of weld lines and their locations should be modeled before tool steel is cut; production trials on cavity pressure transducers can then validate predicted fill patterns.
The principal difference from neat PBT is dimensional behavior in molded parts. Unfilled PBT typically shows mold shrinkage of 1.5% to 2.0% according to ISO 294-4, while the 15 wt% glass-fiber grade reduces mold shrinkage to 0.4% to 0.8%. Cross-flow shrinkage may remain 0.2% to 0.4% above flow-direction shrinkage due to fiber orientation, but the resulting warpage is moderate. A 30 wt% glass-fiber PBT compound suppresses mold shrinkage further, often into the 0.2% to 0.5% range, yet increases density, surface roughness, and anisotropic warpage in flat parts. The following class-reference matrix summarizes the property gradient.
| Property and test method | Neat PBT class | 15 wt% GF PBT class | 30 wt% GF PBT class |
|---|---|---|---|
| Density, ISO 1183-1 | 1.30 g/cm³–1.32 g/cm³ | 1.40 g/cm³–1.44 g/cm³ | 1.52 g/cm³–1.56 g/cm³ |
| Tensile stress at break, ISO 527-2 | 50 MPa–60 MPa | 90 MPa–105 MPa | 120 MPa–140 MPa |
| Flexural modulus, ISO 178 | 2.5 GPa–3.0 GPa | 5.0 GPa–6.0 GPa | 9.0 GPa–10.0 GPa |
| HDT/A, ISO 75-2 | 50°C–60°C | 200°C–210°C | 205°C–220°C |
| Notched Charpy, ISO 179-1/1eA | 3 kJ/m²–4 kJ/m² | 4 kJ/m²–6 kJ/m² | 7 kJ/m²–9 kJ/m² |
| Mold shrinkage, ISO 294-4 | 1.5%–2.0% | 0.4%–0.8% | 0.2%–0.5% |
For relay bases, terminal blocks, automotive sensor housings, and small motor brackets, the 15 wt% glass-fiber grade provides a balance between creep resistance and moldability in multi-cavity tools. Linear coefficient of thermal expansion measured by ISO 11359-2 in the flow direction is typically 30 × 10⁻⁶ K⁻¹ to 50 × 10⁻⁶ K⁻¹, compared with 90 × 10⁻⁶ K⁻¹ to 120 × 10⁻⁶ K⁻¹ for neat PBT, which reduces terminal-position drift during temperature cycling. Gate placement should be selected to orient fibers along the largest dimension of terminal slots; end-gated tensile bars and center-gated plates will produce different anisotropic shrinkage and modulus values, and dimensional tests must be performed on production-gated specimens rather than standard edge-gated test plaques. The material is not a low-shrinkage liquid-crystal polymer, and flatness requirements below 0.1 mm across spans longer than 100 mm may require selective gate relocation, optimized packing pressure, or post-mold fixturing during cooling.
Compliance with EU RoHS Directive 2011/65/EU recast requires screening according to IEC 62321 methods; carbon black and nigrosine colorants in a black PBT compound do not inherently contain restricted heavy metals but must be verified because pigments can carry trace lead or cadmium. XRF screening under IEC 62321-3-1:2013 should be followed by destructive confirmation for lead and cadmium using IEC 62321-5:2013 when XRF signals approach the detection limit. REACH Candidate List obligations apply at 0.1% w/w per article under Article 33; the certificate of analysis and supplier declaration should be checked for each lot. UL 94 flammability classification is specific to the color and minimum thickness listed in the UL Yellow Card file; black grades with carbon black can require a lower limiting thickness to maintain the same class as a natural or colored version. Users should not assume a flame-retardant package from the BK suffix, which denotes black color rather than a V-0 or HB rating.
Electrical properties are not graded by the BK suffix. Comparative tracking index should be measured under IEC 60112 on 3 mm plates, and dielectric strength under IEC 60243-1 at the intended post-mold thickness; values in glass-filled PBT generally depend on plate thickness, fiber content, and moisture uptake. For electrical-connector compliance, the final molded component must be tested with the terminal insert installed, because the metal insert acts as an internal electrode and can reduce breakdown voltage if void-free encapsulation is not achieved.
Chemical resistance is similar to unfilled PBT in dilute acids, aliphatic hydrocarbons, alcohols, and many automotive fuels at ambient temperature, but continuous exposure to hot water, steam, strong alkaline solutions, and some chlorinated solvents can hydrolyze or swell the matrix. Glass-fiber sizing hydrolysis is the primary long-term degradation mechanism in hot ethylene glycol-water mixtures; tensile strength retention should be evaluated by immersion testing under ISO 22088 or the relevant automotive coolant specification. Published data for the 4815 BK grade under coolant aging conditions is limited, and compatibility trials at 90°C or above are recommended when metal inserts, hydrolysis-resistant stabilizers, or weld-line regions are present.
When the 4815 BK compound replaces a 30% glass-fiber PBT in a thin-wall connector housing, the lower glass content improves melt-front progression in 0.4 mm wall sections and permits lower packing pressure, but it also reduces flexural modulus by approximately 40% relative to the higher-filled material. The end-use decision should therefore compare ISO 178 flexural modulus and ISO 179-1/1eA impact values at the final wall thickness with the dimensional stability requirements of the finished assembly. Short-shot defects in such thin sections may require melt temperatures near 270°C and injection velocities up to 150 mm/s; however, the increased shear heating from narrow gates and hot-runner tips must not extend total melt residence time beyond 5 minutes. Under these constraints, the 15 wt% glass-fiber grade typically offers more consistent surface quality and lower internal stress than a 30 wt% glass-fiber grade in the same tool, while retaining sufficient stiffness for connector insertion force retention when terminal retention features are designed with draft angles above 0.5°.