| HS Code | 542239 |
| Material | Polybutylene terephthalate (PBT) |
| Reinforcement | Glass fiber |
| Glass Fiber Content | 30% |
| Density | 1.53 g/cm³ |
| Tensile Strength At Break | 120 MPa |
| Elongation At Break | 2.0% |
| Flexural Modulus | 8000 MPa |
| Flexural Strength | 180 MPa |
| Notched Izod Impact Strength | 8 kJ/m² |
| Heat Deflection Temperature At 1 82 Mpa | 200 °C |
| Melting Point | 225 °C |
| Water Absorption | 0.07% |
| Molding Shrinkage | 0.2–0.8% |
| Flammability Rating | UL94 V-0 |
| Processing Method | Injection molding |
As an accredited Chang Chun LONGLITE® PBT+GF 3030-111 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Chang Chun LONGLITE® PBT+GF 3030-111 is supplied in 25 kg moisture-proof bags, securely palletized for industrial handling and storage. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with palletized 25 kg bags of Chang Chun LONGLITE® PBT+GF 3030-111, shrink-wrapped and securely stowed for ocean shipment. |
| Shipping | Chang Chun LONGLITE® PBT+GF 3030-111 is shipped as non-hazardous, moisture-sensitive, 30% glass-fiber-reinforced PBT pellets in sealed 25 kg moisture-barrier bags, palletized and shrink-wrapped. It is not regulated for transport. Use standard freight, keep dry and cool, and protect from direct sunlight, punctures, moisture ingress, and contamination. |
| Storage | Store Chang Chun LONGLITE® PBT+GF 3030-111 in a cool, dry, well-ventilated area away from direct sunlight, heat, moisture, and incompatible materials. Keep original bags or containers tightly closed, undamaged, and protected from dust. Avoid prolonged high humidity; use dry, sealed packaging. Follow the manufacturer’s SDS and local regulations for safe handling and storage. |
| Shelf Life | Shelf life is typically 12 months when stored in a cool, dry place in original sealed, unopened packaging. |
Automotive under-hood wire-to-board connector housings, fuse-box base plates, and engine control unit header shells are moulded from Chang Chun LONGLITE® PBT+GF 3030-111 where the vehicle qualification plan imposes damp-heat exposure, oil splash, and thermal shock before dielectric withstanding voltage tests. The compound is supplied with a fixed glass-fibre loading of 30 wt% and a pre-compounded flame-retardant package; the production addition ratio is therefore 100 wt% neat material for all live-contact and terminal retention zones, while clean sprue/runner regrind is limited to 15 wt% maximum and only after drying to a residual moisture content below 0.02 wt%. Addition of further glass fibre, flame-retardant masterbatch, or impact modifier is not recommended because the UL rating and the supplier's traceability file are tied to the delivered formulation. Segment compliance is anchored to USCAR-2 Rev 7 for automotive electrical connector systems, SAE J2030 for connector performance validation, ISO 16750-4 for climatic loads, and material certification is based on UL 94 V-0 at a nominal thickness of 1.5 mm, with comparative tracking index tested according to IEC 60112. Downstream processing is injection moulding on machines with 20:1 to 24:1 L/D general-purpose or low-compression screws; the melt temperature is held between 250 °C and 270 °C, the tool surface temperature is maintained between 80 °C and 100 °C, and hold pressure is set from 60 MPa to 85 MPa for wall sections of 0.8 mm to 1.6 mm. Pre-drying at 120 °C for 4 h to 6 h in a desiccant dryer with a dew point of -40 °C to -30 °C is mandatory; processing above 0.02 wt% moisture triggers hydrolytic degradation in polybutylene terephthalate and produces an abrupt loss in weld-line strength before visible surface defects appear. Terminal product types in this segment include sealed and unsealed engine-harness connector bodies, transmission control unit header frames, fuse-box lower mouldings, and sensor connector shells with integral latch features.
In industrial relay bases and contactor control-circuit housings, the material is selected for dimensional stability at coil-operating temperatures and for flame retardance in equipment that must satisfy end-product enclosure requirements. The moulding formulation uses 100 wt% virgin Chang Chun LONGLITE® PBT+GF 3030-111 in all clearance and creepage boundaries; regrind from clean runners is allowed at 15 wt% maximum but only in terminal cover cavities and non-live support ribs, never across an air gap between coil terminals. Applicable compliance documentation includes IEC 61810-1 for electromechanical elementary relays, IEC 60664-1 for insulation coordination, UL 94 V-0 at 1.5 mm material thickness, and IEC 60112 for proof tracking index. Downstream conversion is multi-cavity injection moulding with a hot-runner system; melt temperature is kept between 250 °C and 265 °C, mould temperature between 70 °C and 100 °C, and hold pressure between 50 MPa and 80 MPa. Gate size is not reduced below 0.8 mm because smaller gates cause fibre jamming and visible flow lines at wall thickness transition points. Residence time at melt temperature is kept below 5 min to limit flame-retardant decomposition; the tool steel should be corrosion-resistant or hard-chrome plated in high-shutoff areas. The grade is not positioned for direct arc interruption zones, and arc chamber segments require end-product arc-erosion validation. Terminal parts include relay base housings, contactor coil formers, auxiliary switch bodies, and rail-mount socket bases.
The limiting process variable in EV charging inlet moulding is anisotropic shrinkage produced by the fixed 30 wt% short-glass reinforcement; the flow-direction shrinkage can be less than half of the transverse shrinkage, so unbalanced gating creates the characteristic flange warpage that prevents proper sealing against the charging coupler. For this reason, the component is moulded from 100 wt% virgin Chang Chun LONGLITE® PBT+GF 3030-111; clean regrind is restricted to 10 wt% maximum and is permitted only in rear support ribs that do not form any IP-rated sealing surface or live-contact wall. The part is processed on injection moulding machines with 22:1 to 25:1 L/D screws, sequential valve-gated hot runners, melt temperature 260 °C to 270 °C, tool temperature 90 °C to 100 °C, and hold pressure 65 MPa to 85 MPa. Pre-drying at 120 °C for 4 h to 6 h to below 0.02 wt% moisture is required before processing; moisture above this threshold reduces molecular weight through hydrolysis and is a more common cause of brittle fracture at the coupler latch than insufficient impact strength. Standards applicable to this segment are IEC 62196-1 for conductive charging systems, UL 2251 for plugs and receptacles for electric vehicles, GB/T 20234.1 for Chinese market charge interfaces, SAE J1772 for conductive charge couplers, and UL 94 V-0 at 1.5 mm material thickness. Terminal product types include Type 2 inlet housings, SAE J1772 connector shells, DC fast-charge connector bodies, and busbar carrier plates. Published independent data on long-term weatherability of this specific grade in outdoor charging enclosures is limited; UV exposure must be managed by part design or coating, and end-product resistance to IEC 62196-1 climate tests should be validated on the finished assembly.
Insert moulding of small-appliance motor coil bobbins and brush card holders from Chang Chun LONGLITE® PBT+GF 3030-111 requires preheated copper-alloy terminal strips at 100 °C to 130 °C to avoid premature skin solidification at the insert interface. The production mixture is 100 wt% neat compound for the coil former body; regrind from sprues and runners is permitted at 20 wt% maximum in the non-creepage support collar, while all terminal separation ribs remain virgin material. The insulation-system qualification is conducted under UL 1446, the appliance safety requirement is IEC 60335-1, and the material flame rating is UL 94 V-0 at 1.5 mm. Injection moulding is performed on vertical or rotary-table insert machines with 18:1 to 22:1 L/D screws, melt temperature 250 °C to 265 °C, tool temperature 60 °C to 80 °C, injection speed medium to limit fibre breakage around terminal slots, and hold pressure 50 MPa to 70 MPa. Terminal components are coil bobbins for universal motors, brush card holders, commutator supports, and winding frame covers.
Miniature circuit breaker actuator levers, trip-bar supports, arc barrier plates, and terminal shields are moulded from the same grade where dimensional stability after thermal cycling and flame retardance under abnormal overload conditions are critical. The material flame rating is UL 94 V-0 at 1.5 mm; the material is used at 100 wt% neat compound in current-carrying isolation zones, while regrind is limited to 15 wt% and is excluded from arc chamber and bimetallic strip support areas. Compliance for the final device is evaluated under IEC 60898-1 for miniature circuit breakers, IEC 60947-2 for industrial circuit breaker ratings, UL 489 for moulded-case circuit breakers, IEC 60112 for comparative tracking index, and IEC 60695-2-11 for glow-wire end-product testing. The moulding process requires melt temperature 255 °C to 270 °C, tool temperature 80 °C to 100 °C, and hold pressure 70 MPa to 85 MPa to control post-mould warpage in long actuator levers. Gate placement is aligned with the functional load axis because the fibre orientation at a gate land below 1.0 mm can reduce bending strength by creating a weld line across the lever cross-section. The material is not recommended for direct arc interruption surfaces; published data for arc erosion of this specific glass-fibre flame-retardant grade is limited, and end-product short-circuit testing according to UL 489 remains mandatory for arc chamber components.
In portable power tools, motor end caps, brush card holders, fan impellers, and trigger bodies are moulded from Chang Chun LONGLITE® PBT+GF 3030-111 when the tool specification requires flame retardance retained after thermal ageing and exposure to lubricant mist. The feeding ratio is 100 wt% neat compound in motor end caps and brush card zones; regrind is accepted at 25 wt% maximum in fan impeller hubs and trigger housings that do not form a primary insulation barrier. Standards applied to the segment are IEC 62841-1 for hand-held motor-operated electric tools, UL 60745 for the North American tool safety route, UL 94 V-0 at 1.5 mm, and IEC 60112 for tracking resistance. Conversion is injection moulding with hot-runner multi-cavity tools, melt temperature 250 °C to 265 °C, tool temperature 60 °C to 80 °C, fill time 0.5 s to 1.5 s for thin-wall regions, and hold pressure 40 MPa to 70 MPa. Because the glass reinforcement breaks under high back pressure, screw rotation is limited to 60 rpm to 100 rpm and back pressure is kept below 0.7 MPa to preserve fibre length and impact resistance. Terminal product types are angle-grinder motor end caps, drill brush card holders, orbital-sander fan impellers, and trigger bodies for corded and cordless tools.
Competitive Chang Chun LONGLITE® PBT+GF 3030-111 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chang Chun LONGLITE® PBT+GF 3030-111 is classified as a 30% glass-fibre-reinforced polybutylene terephthalate injection-moulding grade. The 30-series designation refers to the nominal glass-fibre mass fraction, which is incorporated during melt compounding on a twin-screw extruder with an L/D ratio of at least 32:1 to disperse fibre bundles and reduce unwetted agglomerates. Published lot-specific values for the 3030-111 suffix remain the controlling reference; mechanical and processing ranges stated for the 30% reinforced PBT class are screening data and must not replace a certificate of analysis. The grade is non-flame-retarded and is not specified where a UL 94 V-0 classification at 0.75 mm is mandatory.
The semicrystalline PBT matrix melts near 225°C. Production-scale machines process the material with barrel set-points between 240°C and 270°C; grade-specific values must be extracted from the Chang Chun technical datasheet. Because the compound contains 30% glass fibre, screw and barrel wear on injection units is elevated relative to unfilled PBT. Bimetallic barrels, hardened screw flights, and rockwell-hardened check-ring seats are required for campaigns beyond 20 000 operating hours.
Rheological characterisation for flow simulation uses capillary or slit-die data rather than a single melt-flow index. At 250°C and a shear rate of 1000 s-1, the apparent viscosity of 30% glass-fibre-reinforced PBT commonly falls between 80 Pa·s and 150 Pa·s. At 10 000 s-1, shear-thinning reduces apparent viscosity below 30 Pa·s. Cross-WLF or Bird-Carreau parameters should be fitted over 102–104 s-1 and 230–270°C; uncorrected neat-PBT data underpredicts thin-wall pressure drop because fibres suppress wall slip and raise wall shear stress by 10–15%.
Fibre-orientation modelling employs the Folgar-Tucker equation with a post-compounding fibre aspect ratio of 20–30. Flow-aligned regions of a moulded component typically show a linear thermal expansion coefficient of 20–30 ppm/K between 23°C and 80°C, while transverse regions show 50–70 ppm/K. Thermo-mechanical stress at underhood temperature swings therefore depends on local orientation. Published data for this specific configuration is limited; thermodilatometry on plaques moulded from each lot is required for high-precision dimensioning.
Hydrolysis of the ester backbone is the primary degradation mechanism. Moisture uptake accelerates above 60% relative humidity; granulate is dried in a desiccant-bed dryer with a dew point of -40°C or lower at 120°C for 4 h to reach a residual moisture content below 0.02%. Hoppers are purged with dry air and opened no more than 30 min before processing. At 0.05% residual moisture, visible splay and measurable notched impact loss occur.
Barrel settings are bounded at the lower end by the crystallite melting point of PBT near 225°C and at the upper end by thermal degradation accelerated above 280°C. A medium-sized reciprocating-screw machine is configured with feed zone at 230–240°C, compression zone at 250–260°C, metering zone at 250–260°C, and nozzle at 250–270°C. Mould temperature is held between 80°C and 100°C; below 60°C crystallinity is insufficient, while above 110°C cycle time and ejection sticking increase sharply.
The screw compression ratio is maintained between 2.0:1 and 2.5:1, and back pressure is set between 0.3 MPa and 0.7 MPa. Sustained back pressure above 1.0 MPa increases fibre attrition and degrades impact response. Cushion position is held between 2 mm and 5 mm; melt-viscosity differences between lots are compensated by temperature adjustment within the degradation boundary rather than by moving screw speed outside 50–100 rpm without rheological verification.
Drying kinetics are diffusion-limited. At 120°C, a bed depth of 50 mm and a dry-air flow rate of at least 3.5 m³/h per kg are required to reduce moisture from 0.20% to 0.02% in 4 h. In tropical moulding environments above 30°C and 80% relative humidity, open granulate can regain 0.02% moisture within 15–20 min; direct vacuum loading from dryer to hopper is therefore necessary. Dry-air systems with dew points above -20°C are insufficient for holding 0.02% moisture and are a recurring cause of lot-to-lot impact shift.
Flow-induced fibre orientation produces anisotropic mould shrinkage that is treated as a tensor field rather than a single isotropic factor. Under ISO 294-4, flow-direction shrinkage for 30% glass-fibre-reinforced PBT typically lies between 0.3% and 0.7%; transverse shrinkage lies between 0.8% and 1.2%. Melt-front meeting lines, rib intersections, and restricted gates create local orientation gradients that shift local shrinkage by up to 0.3 percentage points. Coplanarity below 0.1 mm on connector shrouds therefore requires three-dimensional warpage simulation with measured fibre-orientation tensors.
Tooling tolerances follow the same anisotropy. Gate diameters below 1.0 mm restrict packing and increase both shrinkage and warpage. Edge gates of 1.5–2.0 mm or sequential valve gates are preferred above 120 mm flow length. Vent depths are held at 0.015–0.025 mm; deeper venting flashes with low-viscosity lots, while shallower venting traps gas and produces burn marks at fibre-rich flow fronts.
The table contains class-reference values for unfilled PBT, 20% glass-fibre-reinforced PBT, and the 30% reinforcement class of LONGLITE PBT+GF 3030-111. The listed values follow the indicated standard methods but are not lot-specific release limits; certificates of analysis remain mandatory for production qualification.
| Property | Test method | Unfilled PBT | PBT+GF 20% | PBT+GF 30% class |
|---|---|---|---|---|
| Density | ISO 1183-1 | 1.31 g/cm³ | 1.45 g/cm³ | 1.52–1.55 g/cm³ |
| Tensile modulus | ISO 527-2/1A | 2600 MPa | 7000 MPa | 9500–10500 MPa |
| Tensile strength | ISO 527-2/1A | 55 MPa | 110 MPa | 120–135 MPa |
| Flexural modulus | ISO 178 | 2500 MPa | 6000 MPa | 8500–10000 MPa |
| Charpy notched impact | ISO 179-1/1eA | 4 kJ/m² | 8 kJ/m² | 7–10 kJ/m² |
| HDT/A at 1.8 MPa | ISO 75-2 | 55°C | 195°C | 200–215°C |
| Mould shrinkage flow | ISO 294-4 | 1.5–2.0% | 0.5–0.9% | 0.3–0.7% |
| Mould shrinkage transverse | ISO 294-4 | 1.5–2.0% | 0.8–1.2% | 0.8–1.2% |
Published data for the exact 3030-111 configuration is limited to the manufacturer’s certificate of analysis. The comparative table isolates the main differences: reinforcement raises tensile modulus by approximately 3–4×, reduces flow-direction shrinkage by approximately 60–80%, and shifts HDT/A from below 60°C to above 200°C. These improvements are accompanied by lower flow length and higher machine wear burden.
Candidate applications are those requiring heat-deflection temperature above 200°C, tensile modulus above 9 GPa, and reduced mould shrinkage relative to unfilled PBT. Electrical terminal blocks, relay sockets, structural sections of connector housings, motor brush holders, sensor brackets, and underhood electrical enclosures are screened with this grade. Dry-air continuous service at 150°C is a reasonable boundary; short peaks to 180°C are tolerated only briefly and reduce creep resistance under load. Continuous exposure to hot water above 60°C or to ethylene glycol/water coolant at 105°C requires hydrolysis-stabilized variants and validation under IEC 60068-2-30 or OEM-specific coolant immersion.
Electrical classification is supply-package dependent. The comparative tracking index of 30% glass-fibre-reinforced PBT commonly ranges from 250 V to 400 V under IEC 60112; the exact value for 3030-111 must be taken from the supplier datasheet because stabilizer and mould-release additives shift tracking resistance. Under UL 94, a non-flame-retarded glass-filled PBT specimen at 0.75 mm is typically classified as HB. The grade is excluded from uninsulated live parts requiring V-0 at 0.75 mm, unless separation, shielding, or a flame-retarded variant is specified. Glow-wire behaviour under IEC 60695-2-11 is thickness- and colourant-dependent and is verified on production-coloured specimens.
Field failure modes on production-scale injection lines are dominated by gate blush, fibre-rich weld lines, and post-moulding warpage. Weld-line tensile strength in 30% glass-fibre-reinforced PBT is typically 50–60% of the reinforced bulk strength because glass fibres do not bridge the melt front. Weld lines are therefore positioned away from snap-fit retention features, or sequential valve gating is used. Mould temperatures above 90°C and injection speeds above 80 mm/s reduce visible glass-fibre bloom on polished surfaces, although deceleration across ribs can increase flow-mark depth.
Valve-gated hot-runner systems with nozzle bores below 2.5 mm can generate wall shear rates exceeding 10 000 s-1. Viscous dissipation then raises local melt temperature by 15–30°C above the nozzle set-point. The permissible residence time at 260°C falls to approximately 8–10 min before tensile strength loss exceeds 5%. Multicavity tools with unbalanced runner layouts should be checked by short-shot thermography or pressure-trace analysis; a cavity-to-cavity melt temperature spread greater than ±5°C triggers sequential valve-gate actuation or runner insert replacement. Hot-runner channels are polished to an Ra below 0.4 µm to reduce stagnant-layer residence time.
The machine nozzle is fitted with a shut-off mechanism. Decompression distance is limited to 3 mm; larger decompression draws air into the melt stream and produces surface splay. Hot-runner manifold temperature is set 5–10°C above the nozzle but below 280°C. Start-up includes a 10–15 min soak at reduced pressure before injection to avoid cold-stab shearing of the glass-filled melt and to prevent check-ring fracture on the first shot.
Notched impact strength of glass-reinforced PBT is a direct function of average post-moulding fibre length. Chopped glass strands enter compounding at a nominal length of 3–4 mm; after compounding and injection moulding, the number-average length commonly falls to 200–350 µm. Screws with compression ratio above 2.8:1 or sustained back pressure above 1.0 MPa produce excessive attrition, shifting fracture from fibre pull-out to matrix-dominated brittle crack growth. The resulting Charpy notched impact loss can reach 20–30% relative to a low-shear screw. This effect is batch-specific and is detected by comparing impact bars moulded at the beginning and end of a 24 h production run.
Thin-wall spiral flow length at 1.0 mm wall and 100 MPa injection pressure is approximately 180–250 mm for this reinforcement class. Below 1.0 mm, filling pressure rises exponentially and the process becomes sensitive to gate freeze-off and fibre jamming in runner turns. On hydraulic machines with clamp force below 800 kN, short-shot defects occur when nozzle pressure drop exceeds available specific pressure by more than 15 MPa. If measured nozzle melt temperature already exceeds 275°C, the gate is enlarged to 1.5–2.0 mm or a direct hot-runner gate is substituted; raising barrel temperature further is excluded by the degradation boundary.
If screw recovery time exceeds 3 s and target cycle time is below 20 s, plasticating capacity is assessed before increasing screw speed above the fibre-attrition boundary. Venting lanes are cleaned every 8 h to remove glass-fibre bloom that blocks gas evacuation. A blocked vent increases cavity gas pressure and produces short-shot or burn-mark defects in thin ribs; the corresponding void content in thick sections is detectable by micro-CT or density measurement under ISO 1183-1.
Chang Chun LONGLITE PBT+GF 3030-111 shares the 30% glass-fibre mass fraction with other 30-series grades but is differentiated through the numerical suffix, which may encode a specific stabilization, flow-modification, or mould-release package. Published data for the exact 3030-111 configuration is limited to the Chang Chun technical datasheet and certificate of analysis. In production, the practical distinctions from adjacent 30% glass-filled grades appear as a shift in melt-volume-flow rate at 250°C/2.16 kg, a changed ejection behaviour on polished cores, and a different moisture-uptake rate after drying. Against unfilled PBT, it raises flexural modulus by approximately 3–4× and reduces isotropic shrinkage by approximately 60–80%; against a 20% glass-fibre grade, it increases tensile strength by 10–20% and reduces transverse warpage but exhibits shorter spiral flow and higher machine wear burden.
Compliance is confirmed from the supplier declaration for the specific batch. The grade is evaluated for EU RoHS Directive 2011/65/EU Annex II restricted substances by screening methods such as IEC 62321-5 for cadmium, IEC 62321-6 for lead, and IEC 62321-8 for phthalates. REACH Regulation 1907/2006 Article 33 disclosure applies when any candidate-list substance exceeds 0.1% by mass in the article. UL certification, SVHC content, and food-contact status must be obtained from Chang Chun for each production lot before assembly qualification.
The following compliance matrix summarises the minimum evidence required for the 3030-111 grade when used in industrial and electrical assemblies.
| Assessment | Reference standard or method | Required evidence |
|---|---|---|
| Restricted substances | EU RoHS 2011/65/EU Annex II; IEC 62321 series | Supplier declaration per batch |
| SVHC disclosure | REACH 1907/2006 Article 33 | Lot-specific concentration check |
| Flammability class | UL 94 at 0.75 mm | Yellow-card or equivalent for exact grade |
| Comparative tracking index | IEC 60112 | Grade-specific CTI in volts |
| Residual moisture | ISO 15512 Method B or equivalent | Below 0.02% before moulding |