| HS Code | 497563 |
| Density | 1.44 g/cm³ |
| Glass Fiber Reinforcement | 10% |
| Flame Retardant | Yes |
| Molding Shrinkage | 0.2–0.4% |
| Tensile Strength | 60 MPa |
| Elongation At Break | 2% |
| Flexural Modulus | 3.0 GPa |
| Notched Izod Impact Strength | 4 kJ/m² |
| Heat Deflection Temperature At 1 82 Mpa | 75 °C |
| Ul94 Flammability Rating | V-0 |
| Volume Resistivity | 1.0E+15 Ω·cm |
| Dielectric Strength | 20 kV/mm |
| Arc Resistance | 120 s |
| Water Absorption | 0.10% |
As an accredited Chang Chun LONGLITE® PBT-FR 2100-104B factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Chang Chun LONGLITE® PBT-FR 2100-104B is packed in 25 kg moisture-proof paper bags, palletized and shrink-wrapped. |
| Container Loading (20′ FCL) | 20′ FCL loading of Chang Chun LONGLITE® PBT-FR 2100-104B: palletized bags, shrink-wrapped, evenly distributed and secured for safe ocean transport. |
| Shipping | Chang Chun LONGLITE® PBT-FR 2100-104B is shipped as flame-retardant PBT resin pellets in sealed moisture-barrier bags, packed in cartons/boxes on pallets. Store and transport in a cool, dry, ventilated area away from direct sunlight, heat, and moisture. Normally not classified as dangerous goods; follow local regulations. |
| Storage | Store Chang Chun LONGLITE® PBT-FR 2100-104B in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep packaging tightly closed and palletized to prevent moisture ingress and physical damage. Avoid contact with strong oxidizers and acids; follow the SDS and local regulations. |
| Shelf Life | When stored cool, dry, and unopened, Chang Chun LONGLITE® PBT-FR 2100-104B typically has a shelf life of about two years. |
In DIN rail terminal block manufacturing and PCB-mounted power connector bodies, the selection of unfilled flame-retardant polybutylene terephthalate rests on the requirement to fill thin insulating walls without excessive pack pressure while retaining dielectric integrity after thermal cycling. LONGLITE® PBT-FR 2100-104B is processed as a neat pellet stream at 100 wt%; the formulation addition ratio is therefore 100 wt% resin, with regrind from sprue, runner, and rejected cavities limited to ≤20 wt% of total shot mass. Higher regrind ratios reduce the comparative tracking index value measured under IEC 60112 and increase the probability of weld line fracture during screw-terminal torque insertion. No secondary flame-retardant masterbatch or diluting non-FR PBT is added, because the compound is supplied with the flame-retardant package already dispersed. If colour masterbatch is required, it is limited to ≤2 wt% of a PBT-compatible carrier and counted within the regrind fraction. The material must be dried in a desiccant dryer at 120–140 °C for 4–6 h to a moisture level below 0.02 wt%; residual moisture above that threshold hydrolyses the ester linkages during plastication, producing silver streaking and a measurable drop in tensile elongation at break under ISO 527-2.
Compliance for this sector is anchored to IEC 60947-7-1 for terminal blocks, IEC 60664-1 for creepage and clearance coordination, and UL 94 V-0 for flammability classification according to the UL Yellow Card thickness. Glow-wire evaluation under IEC 60695-2-11 is specified when the terminal block is installed in unattended equipment. Injection moulding on production lines typically uses a three-zone screw with an L/D ratio of 20:1 to 25:1, a melt temperature of 240–260 °C, a tool temperature of 60–100 °C, and a back pressure of 0.3–0.7 MPa. Higher melt temperatures above 260 °C accelerate flame-retardant degradation, generating black specks and acid by-products that corrode polished tool surfaces. Terminal product types include DIN rail feed-through terminal blocks, plug-in PCB connectors, sensor connector bodies, and isolation barriers in instrumentation housings.
Miniature circuit breaker internal inserts must tolerate the pressure pulse and ionised gas environment associated with short-circuit interruption tests under IEC 60898-1 and IEC 60947-2. The component is moulded from 100 wt% LONGLITE® PBT-FR 2100-104B with post-industrial regrind held to ≤15 wt% if the insert is directly adjacent to the arc chamber. At 20 wt% regrind, batch observations on high-cavitation tooling show a wider distribution of notched impact results under ISO 179-1/1eA, which increases the rejection rate after automatic riveting of contact carriers. No glass reinforcement is added, because the resulting loss of arc-track resistance would require complete revalidation under the short-circuit test sequence. The polymer phase is not diluted with non-FR PBT, and no external flame-retardant masterbatch is added.
The dominant process conflict is weld-line formation at the narrow insulating fins that separate moving contacts. These fins have a wall thickness commonly between 0.5 mm and 0.8 mm, and the flow front must travel through multiple gates around steel pins. If the tool temperature is kept below 70 °C, the melt freezes at the weld line before molecular diffusion establishes a robust knit, producing low fracture resistance during screw torque and thermal cycling. Raising the tool temperature to 90–100 °C and increasing injection velocity to fill the fins in less than 0.5 s reduces the visible weld line and improves knit strength. However, flash formation becomes problematic at vent depths above 0.02–0.03 mm because unfilled flame-retardant PBT has a lower melt viscosity than glass-filled grades, and small overpacking excursions force material into the vent lands.
Flammability classification under UL 94 V-0 must be maintained at the section thickness used in the insulating fin, and the material certificate should be checked against the UL Yellow Card. Arc resistance under IEC 61621 and comparative tracking index under IEC 60112 are used for insulating parts exposed to high electric stress. Drying and melt residence time are critical: barrel residence time should not exceed 5 min, and the hot-runner manifold should be designed without stagnation zones. Terminal product types include arc chamber inserts, moving contact supports, rotary switch insulators, and auxiliary contact housings.
| Downstream part | Primary product standard | Test designation | Moulding acceptance basis |
|---|---|---|---|
| DIN rail terminal blocks | IEC 60947-7-1 | IEC 60695-2-11 | No ignition at specified glow-wire temperature; UL 94 V-0 at Yellow Card thickness |
| Miniature circuit breaker inserts | IEC 60898-1, IEC 60947-2 | IEC 60112 | CTI certificate value; no post-test tracking path |
| Relay coil formers | IEC 61810-1 | IEC 60243-1 | Breakdown voltage above end-product insulation requirement |
| DC charging inlet housings | IEC 62196-1, UL 2251 | IEC 60112 | CTI as per design clearance; UL 94 V-0 rating retained |
| Heating appliance terminal carriers | IEC 60335-1 clause 30.2.3 | IEC 60695-2-12, IEC 60695-2-13 | No sustained flaming; afterflame ≤30 s where required |
Relay coil former production is governed less by ignition resistance than by circumferential cracking when the wound copper coil is impregnated with unsaturated polyester or epoxy encapsulants and cured at 120–150 °C. LONGLITE® PBT-FR 2100-104B is used at 100 wt% neat pellet feed, with regrind held to ≤15 wt% when the bobbin flange thickness falls below 0.8 mm. The addition of external release agents or low-molecular-weight processing aids is not recommended for coil formers that will undergo hot potting because unreacted additive migration can reduce adhesion of the encapsulant and produce an interfacial void that becomes a partial-discharge site. Amine-containing mould-release agents are specifically incompatible because they accelerate ester hydrolysis and can cause stress cracking at the flange root. Downstream production involves injection moulding of the bobbin, automatic winding at controlled tension, insertion of the core, and thermoset encapsulation. Compliance is based on IEC 61810-1 for electromechanical elementary relays, IEC 60243-1 for electric strength of insulating materials, and UL 1446 when the coil former is part of a recognised insulation system. Terminal product types include miniature relay coil bobbins, solenoid coil formers, timer motor bobbins, and contactor coil bodies.
At DC charging interfaces, the insulating housing must satisfy creepage and clearance requirements under IEC 62196-1, while the North American product listing applies UL 2251. The limiting electrical property is often comparative tracking index under IEC 60112, because conductive dust and de-icing salt on charging connector faces can create surface leakage currents. LONGLITE® PBT-FR 2100-104B is injected as the sole polymer phase at 100 wt%; regrind is limited to ≤20 wt% for non-live internal components and ≤10 wt% for live parts where the moulded-in contact sockets are not overmoulded. Dilution with non-flame-retardant PBT or glass-filled PBT is prohibited without repeating the full UL 94 and IEC 60112 validation programme, because the glass phase can lower the tracking index and create micro-voids at fibre ends.
The production process for charging inlet housings uses sequential valve gating to prevent knit lines around the terminal sockets. The melt temperature is held at the lower end of the processing window, 240–250 °C, to minimise thermal degradation of the flame-retardant package during long filling paths. Tool temperature is set at 90–100 °C with pressurised water units to allow crystallisation of the thin wall sections around the contact chambers. Barrel residence time should not exceed 5 min, and start-up purges should be discarded until the melt appears free of amber discoloration. In production equipment, screw speed is limited to 80–120 rpm to avoid excessive shear heating of the flame-retardant polyester.
Published comparative tracking index data for this specific grade under salt-fog exposure are limited; the lot certificate value determined by IEC 60112 must be fixed into the design verification plan before tooling release. Terminal product types include AC/DC charging inlet housings, coupler bodies, charging station internal insulating plates, and battery disconnect switch housings.
Heating appliance terminal carriers are subjected to glow-wire tests under IEC 60335-1 clause 30.2.3 when the appliance operates unattended. The test method is IEC 60695-2-11, with glow-wire temperatures of 750 °C or 850 °C depending on the carrying current and supervision category. LONGLITE® PBT-FR 2100-104B is processed at 100 wt% neat pellet feed. Regrind addition is limited to ≤15 wt% because repeated heat-and-shear history shortens the polymer chains and alters the melt viscosity; the first evidence is a wider variation in glow-wire ignition time and afterflame time within a moulding batch. External flame-retardant masterbatch addition is not required and is not recommended, because a local excess of flame-retardant particles can produce surface roughness that retains carbonaceous residues during the glow-wire test.
The downstream process uses injection moulding with hot runner systems for multi-cavity production of thin-walled terminal carriers. The mould temperature is set to 80–100 °C so that the part reaches sufficient crystallinity before ejection and does not distort during later exposure to radiant heat from the heating element. Venting is critical: insufficient venting at the end of the fill path creates dieseling marks that become preferential ignition points under IEC 60695-2-12. Vent depth is maintained at 0.02–0.03 mm, and vacuum assist is sometimes used to remove volatile by-products. Terminal product types include hair dryer heating element carriers, electric kettle base terminal blocks, infrared heater terminal housings, and fan heater internal switch mounts.
Small motor brush holders and rocker switch bases use the same neat pellet feed at 100 wt% with regrind limited to 20 wt% because the insulating sections are relatively thick and do not face the same thin-wall glow-wire burden as appliance terminal carriers. Compliance follows IEC 60335-1 for appliance motors and UL 94 V-0 for switch bodies. Injection moulding parameters follow the drying and melt-temperature window described for terminal blocks, with the main production limitation being ejection pin deflection or push-through when the tool is opened before the part has cooled below 90 °C. Terminal product types include brush holder insulating caps, rocker switch bases, slide switch housings, and small motor commutator covers.
Competitive Chang Chun LONGLITE® PBT-FR 2100-104B prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Chang Chun LONGLITE® PBT-FR 2100-104B is an unreinforced flame-retardant polybutylene terephthalate injection-molding grade in the LONGLITE 2100 series produced by Chang Chun Plastics Co., Ltd. The 104B suffix identifies a specific colorant and stabilizer package; the grade is not a general-purpose PBT. The material is supplied for injection molding of electrical and electronic parts, including connector bodies, relay housings, terminal blocks, sockets, switches, and transformer bobbins where a UL 94 flame-retardant classification is required in thin-wall sections. Design and processing personnel should treat the current producer datasheet and yellow card as the controlling specification because lot-specific values may vary with pigmentation and molecular weight distribution.
In the absence of a lot-specific certificate, the material should not be described using values from the broader LONGLITE PBT family. Representative data for unfilled flame-retardant PBT of this class, measured at 23 °C and 50% relative humidity after standardized conditioning, appear in the following table. Values are reported as class ranges and do not replace the manufacturer's grade-specific datasheet.
| Property | Test method | Unit | Typical class range |
|---|---|---|---|
| Density | ISO 1183-1 | g/cm³ | 1.45–1.52 |
| Tensile stress at break | ISO 527-2 | MPa | 55–65 |
| Flexural modulus | ISO 178 | MPa | 2500–2800 |
| Charpy notched impact, 23 °C | ISO 179-1/1eA | kJ/m² | 3–5 |
| Melt volume-flow rate, 250 °C / 2.16 kg | ISO 1133-1 | cm³/10 min | 15–30 |
| Heat deflection temperature, 0.45 MPa | ISO 75-2 | °C | 140–165 |
| Heat deflection temperature, 1.8 MPa | ISO 75-2 | °C | 55–70 |
| Flammability classification at 0.75 mm | UL 94 | class | V-0 |
The property differences between standard unfilled PBT and the flame-retardant version are not limited to density. The flame-retardant package shifts melt viscosity and can reduce notched impact and weld-line strength. Therefore, grade-specific melt viscosity curves should be used for mold-filling simulation. If the 2100-104B datasheet differs from the class ranges above, the datasheet governs.
Pre-drying is a binding condition. Polybutylene terephthalate undergoes hydrolytic degradation when residual moisture exceeds 0.02% by weight at melt temperature. A dehumidifying hopper dryer operating at 120 °C for 4 h, or at 80 °C for 8 h, with a dew point of -30 °C or below, is required when the material has been exposed to ambient humidity above 60%. Lot-to-lot moisture content in unopened packaging should be verified before first use. On production lines, feed hoppers with dry-air purge and closed conveying reduce moisture re-uptake. Parts molded from inadequately dried material show silver streaks, gas splay, and sharp elongation loss.
Barrel temperatures from 240 °C to 270 °C are typical. The nozzle should be controlled at 250–260 °C, and the mold surface should be maintained at 60–90 °C to promote crystallization and sufficient part ejection. Melt temperature measured by nozzle pyrometer should not exceed 270 °C for extended periods. The flame-retardant system is thermally sensitive; residence time above 260 °C should be kept below 5 min. Extended residence or high shear can produce yellowing, brown streaks, mold deposits, and loss of UL 94 consistency.
Injection velocity for unfilled FR PBT is typically set at 50–150 mm/s. Thin-wall parts with nominal wall thickness from 0.75 mm to 1.50 mm require fill times of 0.5–1.5 s. High velocity settings above the upper range can produce jetting and gate blush, especially at pinpoint gates. Hold pressure should be 50–70% of peak injection pressure, sealed by adequate hold time; insufficient hold pressure causes sink marks and voids. Back pressure should be kept in the range of 0.3–0.7 MPa. Clamp force requirements for multicavity parts are estimated at 3.5–5.0 kN/cm² of projected area, but final values must be confirmed by mold filling and pressure drop analysis.
Machines with general-purpose screws of L/D 18:1–22:1 and compression ratio 2.0:1–2.5:1 are suitable. A reverse-cut check ring reduces material stagnation. Purging after interruption should use unfilled PBT purge compound or polycarbonate purge compound; residues of polyamide or polyolefin must be removed because they degrade or delaminate at PBT processing temperatures. If reprocessing through a twin-screw extruder is attempted to blend regrind or color, the barrel temperature should be limited to 260 °C and residence time must be short. The producer should be consulted before adding downstream compounding steps.
The material is typically listed as V-0 at 0.75 mm on the producer's UL 94 yellow card. Some subgrades may carry a 0.4 mm listing; the 2100-104B colorant package must be verified because pigmentation can influence flame-retardant performance. Design at 0.4 mm is not automatically covered by a 0.75 mm listing. Thin-wall geometry changes flow length, and the flame-retardant phase may be sheared in gate regions, altering local flame-retardant performance. Published data for this specific configuration at 0.4 mm is limited; end-product flame tests are required for production approval.
Knit lines are a critical concern. In FR PBT, knit-line strength is generally lower than in non-FR PBT, and published data for 2100-104B knit-line mechanical properties is limited. For multiple gates, cavity filling should be arranged to move weld lines away from snap-fit arms and high-stress bosses. Hot-runner systems with gate diameters below 0.8 mm create high shear rates; valve-gated hot runners are preferred when gate diameters are less than 1.0 mm.
Regrind use alters molecular weight distribution and can affect the UL 94 classification. A regrind level up to 15% is sometimes used in non-safety-critical parts, but published data for 2100-104B with regrind is limited. The producer should be contacted when reclaimed material is used in parts that must retain V-0 at 0.75 mm. The flame-retardant package also influences color and opacity; visual color standards should be established using the exact 104B suffix, not a general natural PBT reference.
Standard unfilled LONGLITE PBT grades without flame retardant typically show density in the range of 1.30–1.33 g/cm³ and higher tensile elongation. The flame-retardant grade raises density, reduces notched impact, and modifies shrinkage. Shrinkage for unfilled FR PBT is generally 1.2–1.6% in the flow direction and 1.4–1.8% transverse; tool designers should use grade-specific shrinkage data. Compared with glass-filled LONGLITE PBT, the unfilled FR grade has lower stiffness and strength but lower warpage in flat electrical parts. Glass-filled PBT can exceed 6000 MPa flexural modulus, while the unfilled FR PBT class remains near 2500–2800 MPa. This difference shifts snap-fit design: lower stiffness may reduce insertion force but also reduces retention force at the same deflection.
Glass-filled LONGLITE PBT grades are specified where rigidity and elevated heat deflection under load are required. The addition of glass raises flexural modulus, tensile strength, and creep resistance but introduces anisotropic shrinkage and warpage. Unfilled PBT-FR 2100-104B is selected for flat, thin-walled connectors where warpage control and electrical-tracking performance are more important than maximum stiffness. When the application requires high pin retention force, a glass-filled grade is typically selected; when moldability, low warpage, and surface appearance are controlling, the unfilled FR grade is evaluated.
Halogen-free flame-retardant PBT systems differ in key electrical properties. Phosphorus-based or metal phosphinate systems often show comparative tracking index values above 600 V, while halogenated FR systems may fall in the 250–400 V range depending on synergist concentration. The CTI value for 2100-104B must be taken from the producer datasheet because the flame-retardant chemistry is not specified in public sources. The choice between halogenated and halogen-free FR PBT affects density, melt viscosity, and mold-corrosion behavior; mold steel selection should consider potential acid evolution if decomposition occurs.
Other FR PBT grades in the 2100 series may differ by flow length, colorant package, and UL 94 minimum thickness. The 104B suffix is not interchangeable with natural or black versions when color and regulatory evidence are part of the approval package. Flame-retardant PBT shows shear-thinning behavior, but the low-shear viscosity is more sensitive to flame-retardant particle packing than standard PBT. Mold-filling simulation for 2100-104B should use Cross-WLF coefficients fitted from capillary rheometry, not generic PBT values. Capillary rheometry data from the producer, if available, is preferred; without it, initial simulations may be based on the class range but should be adjusted after first-shot short-shot studies. The melt volume-flow rate range in the property table is not sufficient for gate design.
Flame-retardant performance is only one element in material acceptance. For electrical and electronic applications, IEC 62368-1 may require flammability classification, comparative tracking index, and resistance to ignition under fault conditions. The UL 94 V-0 classification from the material supplier is a material-scale screening test, not a substitute for end-product fire enclosure testing. The manufacturer's yellow card and certificate of compliance should be reconciled with the actual production lot and colorant suffix.
RoHS compliance under Directive 2011/65/EU is documented at the homogeneous material level using IEC 62321 methods. The supplier declaration for LONGLITE PBT-FR 2100-104B should specify the tested lot, date, and test method. Under REACH Regulation (EC) No 1907/2006, Article 33 communication triggers if the material contains an SVHC above 0.1% by weight of the homogeneous material; the current candidate list and safety data sheet should be checked.
| Requirement | Standard or regulation | Evidence required for this material class |
|---|---|---|
| Flammability | UL 94 | Current yellow card listing V-0 at 0.75 mm or applicable thickness |
| Comparative tracking index | IEC 60112 | Producer datasheet value; CTI class per IEC 60664-1 if applicable |
| Restriction of hazardous substances | Directive 2011/65/EU | Lot-specific test report using IEC 62321 methods |
| SVHC communication | REACH (EC) No 1907/2006 | SDS and SCIP notification where applicable |
| Material marking | ISO 11469 | Producer-specified >PBT-FR< code |
Operational boundaries for this grade include the drying specifications, melt-temperature ceiling, and regrind restrictions already stated. The material is not intended for food-contact applications unless expressly supported by regulatory clearance. The grade should not be combined with amine-based additives or incompatible color concentrates, because these may react with the polyester matrix or flame-retardant system during melt processing. The producer's safety data sheet, datasheet, and UL 94 documentation must be controlled documents within the part approval file.