| HS Code | 157802 |
| Density | 1.30 g/cm³ |
| Melt Volume Flow Rate | 20 cm³/10 min (250°C/2.16 kg) |
| Tensile Modulus | 2600 MPa |
| Tensile Stress At Yield | 55 MPa |
| Tensile Strain At Yield | 3.5% |
| Nominal Strain At Break | 20% |
| Charpy Notched Impact Strength At 23 C | 5 kJ/m² |
| Charpy Notched Impact Strength At 30 C | 4 kJ/m² |
| Heat Deflection Temperature At 1 8 Mpa | 60°C |
| Heat Deflection Temperature At 0 45 Mpa | 150°C |
| Melting Temperature | 225°C |
| Vicat Softening Temperature B | 175°C |
| Water Absorption | 0.4% |
| Molding Shrinkage | 1.6% |
As an accredited Celanese Crastin® Unreinforced PBT S620F20 NC010 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg moisture-barrier bags, palletized; each pallet contains 40 bags (1,000 kg) for industrial handling. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): Dry, clean 20′ FCL loaded with palletized Celanese Crastin® S620F20 NC010 PBT, shrink-wrapped and secured for ocean transport. |
| Shipping | Celanese Crastin® Unreinforced PBT S620F20 NC010 is supplied as natural-color thermoplastic pellets in moisture-barrier bags, lined boxes, or drums, palletized and labeled with product/lot information. Ship dry at ambient temperature, away from heat and moisture, per SDS and applicable transport regulations. |
| Storage | Store Celanese Crastin® Unreinforced PBT S620F20 NC010 in a cool, dry, well-ventilated area in its original sealed packaging. Protect from moisture, direct sunlight, heat, and contamination. Keep away from strong chemicals and odors. Maintain moderate temperatures and avoid humid conditions. Reseal opened containers and dry material per supplier recommendations before processing. Follow the manufacturer’s SDS and local regulations. |
| Shelf Life | Celanese Crastin® PBT S620F20 NC010 has a shelf life of 24 months when stored dry in unopened packaging at ≤30°C. |
Competitive Celanese Crastin® Unreinforced PBT S620F20 NC010 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Celanese Crastin® S620F20 NC010 is an unreinforced polybutylene terephthalate (PBT) grade supplied in natural colour. The designation identifies a medium-flow, non-flame-retarded PBT formulated for injection moulding and, where screw configuration permits, thin-wall extrusion. Because the compound contains no glass fibre or mineral filler, it provides a ductile stress-strain response, a smooth moulded surface, and lower density than filled PBT grades while retaining the rapid crystallisation that separates PBT from polyethylene terephthalate (PET). The material is specified where electrical tracking resistance, hydrocarbon tolerance, low moisture uptake, and post-moulding dimensional behaviour are more important than load-bearing stiffness.
The grade is typically processed by high-speed injection moulding, with part geometries ranging from electrical connectors and relay sockets to appliance housings and automotive interior sensor carriers. In these applications, the unfilled grade competes with PA66, polyoxymethylene (POM), and glass-filled PBT; selection is based on flow behaviour, surface finish, shrinkage, and long-term exposure limits rather than on maximum tensile modulus.
PBT is a semicrystalline aromatic polyester produced by the polycondensation of dimethyl terephthalate with 1,4-butanediol. The S620F20 NC010 grade exhibits a melting temperature of 225 °C under ISO 11357-3. The glass transition is near 45 °C to 60 °C. The melt volume-flow rate is approximately 19 cm³/10 min at 250 °C/2.16 kg when tested according to ISO 1133-1, placing the product in the medium-flow segment of the Crastin PBT range. Density is 1.31 g/cm³ under ISO 1183-1.
| Property | Test standard | Typical value |
|---|---|---|
| Density | ISO 1183-1 | 1.31 g/cm³ |
| Tensile modulus | ISO 527-2 | 2600 MPa |
| Tensile stress at yield | ISO 527-2 | 58 MPa |
| Tensile strain at break | ISO 527-2 | 50 % |
| Flexural modulus | ISO 178 | 2500 MPa |
| Charpy notched impact strength, 23 °C | ISO 179-1/1eA | 4.0 kJ/m² |
| Heat deflection temperature, 0.45 MPa | ISO 75-2/B | 160 °C |
| Heat deflection temperature, 1.8 MPa | ISO 75-2/A | 60 °C |
| Flammability at 3.0 mm | UL 94 | HB |
Water absorption is low compared with aliphatic polyamides. Under ISO 62, room-temperature moisture uptake at 50 % relative humidity remains below 0.3 % for the unfilled PBT class, whereas PA66 can approach 2.5 % under equivalent conditions. This difference stabilises electrical properties and dimensions in humid environments.
Unfilled PBT does not contain glass-fibre orientation effects, but crystallisation and thermal contraction still produce anisotropic mould shrinkage. Published mould shrinkage values under ISO 294-4 for the unreinforced grade are commonly reported as 1.5 % to 2.0 % in the flow direction and 1.6 % to 2.2 % transverse to flow. The exact balance depends on gate location, packing pressure, mould temperature, wall thickness, and gate freeze time.
At mould temperatures below 50 °C, the skin layer freezes before sufficient crystallisation occurs; the part can then relax after ejection and exhibit additional post-moulding shrinkage of up to 0.3 % during uncontrolled storage. Raising the mould temperature to 80 °C increases crystallinity and reduces post-shrinkage but extends cycle time and can aggravate sticking in deep cores. The practical mould-temperature window for dimensional stability is therefore 60 °C to 90 °C for most unfilled PBT moulds.
Warpage in flat connector carriers is produced when fill orientation and differential cooling create an uneven shrinkage field. End-gated rectangular parts with length-to-thickness ratios above 30:1 can develop visible bow if the near-gate and far-gate shrinkage differ by more than 0.2 %. In such geometries, mould-flow simulation using anisotropic PBT shrinkage data is required before tool steel is cut. Compared with 30 % glass-filled PBT, the unfilled grade exhibits higher absolute shrinkage but lower orientation-driven warpage because no high-aspect-ratio fibres are present.
Pre-drying is mandatory for hydrolysis control. PBT is processed from a dehumidified air dryer set at 120 °C for 4 h to 6 h, with a supply air dew point below -30 °C. At pellet moisture levels above 0.02 % by weight, hydrolytic chain scission during melt processing reduces molecular weight and produces visible splay or silver streaks on the moulded surface. Moisture should be verified by ISO 15512 before start-up. A hopper dryer without a desiccant bed does not reliably achieve the required dew point and is not an acceptable substitute for closed-loop dehumidified drying.
Melt temperature should be maintained at 240 °C to 260 °C, with the optimum set point near 250 °C. Residence time at melt temperature should not exceed 5 min; above 270 °C thermal degradation of the ester linkage accelerates, releasing tetrahydrofuran and carbon dioxide and causing black specks, yellowing, and acrid fumes. Screw plastication for a 20:1 to 22:1 L/D general-purpose screw with a compression ratio of 2.5:1 is appropriate. Back pressure is typically 0.3 MPa to 0.7 MPa, and screw speed is set to avoid excessive shear heating.
Injection velocity should be set to fill thin-wall connector cavities in 0.5 s to 1.5 s for wall thicknesses up to 2.0 mm. Slow fill can lead to premature gate freeze-off and elevated packing demand. Injection pressure is commonly 80 MPa to 120 MPa depending on flow length. Holding pressure is set at 60 % to 80 % of injection pressure and maintained until the gate seals to control sink and dimensional consistency.
If dried pellets are exposed to ambient air with relative humidity above 60 % for more than 30 min, moisture regain can be sufficient to reintroduce hydrolysis defects in open hoppers without closed-loop drying. For long-term contact with water above 60 °C, the polyester linkage is subject to hydrolytic degradation even in moulded parts. Published data for this specific grade under hot-water immersion are limited, but the unfilled PBT class is generally not recommended for continuous exposure to 85 °C water or steam because tensile strength retention can fall below 50 % within 1000 h depending on part thickness, water chemistry, and mechanical load. Strong acids, strong alkalis, and amine-based cleaners accelerate the same degradation mechanism and should be avoided in application environments.
The unfilled S620F20 NC010 occupies a distinct position within the Crastin portfolio. Glass-filled PBT grades are selected when tensile modulus above 9000 MPa and heat deflection temperature above 200 °C are required; the unreinforced grade is selected when elongation above 50 %, low mould abrasion, and a smooth surface are more important. Flame-retardant PBT grades provide a UL 94 V-0 rating but commonly exhibit lower tracking resistance and narrower processing windows unless specially formulated.
| Comparison metric | Crastin S620F20 NC010 | 30 % glass-filled PBT | Halogen-free FR unreinforced PBT |
|---|---|---|---|
| Tensile modulus, ISO 527-2 | 2600 MPa | 9500 MPa | 3000 MPa |
| Tensile strain at break, ISO 527-2 | 50 % | 2.5 % | 12 % |
| HDT, 0.45 MPa, ISO 75-2/B | 160 °C | 215 °C | 160 °C |
| Density, ISO 1183-1 | 1.31 g/cm³ | 1.53 g/cm³ | 1.45 g/cm³ |
| Mould shrinkage, flow direction | 1.5 % to 2.0 % | 0.3 % to 0.6 % | 1.8 % to 2.3 % |
| UL 94 rating at 3.0 mm | HB | HB | V-0 |
The comparative values are representative ranges for the material classes and should be verified against current grade-specific datasheets. The unfilled grade also differs from PA66 in moisture sensitivity: PA66 absorbs enough water to shift dimensions and lower tensile modulus in humid environments, whereas the PBT grade remains nearly unchanged below 60 % relative humidity. Against POM, the unfilled PBT offers higher tracking resistance but lower resistance to hot-water and acid exposure; POM is preferred in hot-water pump components.
Electrical connectors and relay sockets manufactured from S620F20 NC010 commonly use wall thicknesses from 0.4 mm to 2.5 mm. The natural PBT grade typically shows a comparative tracking index above 600 V under IEC 60112, which supports creepage-distance reduction in low-voltage connectors. In automotive interior sensor housings, the material is selected for low moisture uptake, low warpage relative to unfilled PA66, and resistance to aliphatic hydrocarbons and mild automotive fluids. Continuous use is limited by the 1.8 MPa heat deflection temperature of 60 °C; the grade is therefore assigned to bracketry and sensor housings where the local air temperature remains below 60 °C unless mechanical load is minimal.